Filling material for gaps between coke oven wall bricks and steel plates and preparation method of filling material
Through the two-way fusion bonding technology of new fillers, the problem of poor gap filling in coke oven repair is solved, high bonding strength and long hanging time are achieved, and the service life of the coke oven is extended.
Patent Information
- Application Number
- CN202410752965.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-12
AI Technical Summary
Existing coke oven repair methods cannot effectively fill the gaps between the steel plates and furnace wall bricks, resulting in poor repair results, short hanging time and inability to extend the service life of the coke oven.
A new type of filler is used, including fused quartz, calcined quartz, aluminum powder, iron powder, FeO, ZnO, CrN and active α-Al2O3, and forms a two-way melting bond with the steel plate and furnace wall bricks through self-propagating high-temperature synthesis technology, using bubbles. Anthocyanine acts as a water-reducing agent to achieve dense filling of materials.
The two-way high bonding strength of the steel plate and furnace wall bricks is achieved, which prolongs the hanging time. The filler has good fluidity and density, which can effectively extend the service life of the coke oven.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of refractory materials for coke oven repair in the steel industry, and in particular relates to a filler for gaps between coke oven wall bricks and steel plates and a preparation method thereof. Background Art
[0002] Coke ovens are complex large-scale industrial kilns, and their construction investment accounts for about 20% of the total investment of the entire coking plant. Their service life directly affects the production cost and economic benefits of coking enterprises. Coke ovens have a long service life, generally about 30 years, and some even reach more than 40 years. However, during the long-term operation, due to the influence of factors such as temperature stress, physical and chemical effects, and mechanical force impact, the furnace body is inevitably damaged, mainly manifested in wall erosion, pitting and falling of the furnace head, cracks in the top bricks, etc., which seriously affect the normal production and service life of the coke oven. Therefore, it is very necessary to reasonably repair the damage to the coke oven. Strengthening coke oven repair and extending the service life of the coke oven has become an important task in the coking industry.
[0003] Coke oven repair methods are divided into cold repair and hot repair. Cold repair methods include wet spraying, smearing, semi-dry spraying, etc. Hot repair methods include ceramic welding and ceramic smearing. Different repair methods are used according to the usage characteristics of different parts of the coke oven, but no matter the cold repair method or the hot repair method, the gap between the outer wall steel plate and the furnace wall brick of the coke oven cannot be effectively maintained. The cold repair hanging time is short, and the repair is only 2 to 3 months, and the gap cannot be filled densely, while the hot repair material cannot be combined with the steel plate, resulting in the gap being burned directly through. Summary of the invention
[0004] In view of the existing problems, the purpose of the present invention is to provide a new type of filler for repairing the gaps between the wall bricks and steel plates of coke ovens and a preparation method thereof, which is characterized in that it can simultaneously form a molten bond with the steel plates and the refractory bricks of the furnace wall, has high bidirectional bonding strength, and can extend the material hanging time for one repair to more than one year. At the same time, the material uses the self-propagating high-temperature synthesis technology to fill the gaps densely.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0006] The invention provides a filler for gaps between coke oven wall bricks and steel plates. The filler raw material components include, by weight percentage: fused quartz: 16%-30%, calcined quartz: 10%-35%, aluminum powder: 10%-15%, iron powder: 7%-20%, FeO: 5%-20%, ZnO: 5%-15%, CrN: 1%-5%, active alpha-Al2O3: 2%-8%, and a water reducer: 0.1%-0.3%.
[0007] As a further improvement of the present invention, the particle size distribution of the fused quartz is 3mm to 5mm, the particle size distribution of the calcined quartz is 1mm to 3mm, the particle size distribution of the aluminum powder is less than 30μm and is not equal to 0mm, the particle size distribution of the iron powder is less than 30μm and is not equal to 0mm, the particle size distribution of FeO is 0mm to 0.5mm and is not equal to 0mm, the particle size distribution of ZnO is 0mm to 1mm and is not equal to 0mm, the particle size distribution of CrN is 0mm to 1mm and is not equal to 0mm, the particle size distribution of active α-Al2O3 is less than 0.088mm, and the particle size distribution of the water reducer is 175 to 185 meshes.
[0008] As a further improvement of the present invention, the water reducing agent is sodium carbonate.
[0009] As a further improvement of the present invention, the filler raw material components include, by weight percentage: fused quartz: 17% to 26%, calcined quartz: 15% to 31%, aluminum powder: 12% to 14%, iron powder: 9% to 15%, FeO: 5% to 15%, ZnO: 7% to 13%, CrN: 3% to 5%, active α-Al2O3: 4% to 7%, and water reducer: 0.1% to 0.2%.
[0010] As a further improvement of the present invention, the filler raw material components include, by weight percentage: fused quartz: 19% to 22%, calcined quartz: 19% to 25%, aluminum powder: 12% to 13%, iron powder: 11% to 13%, FeO: 7% to 12%, ZnO: 8% to 12%, CrN: 4% to 5%, active α-Al2O3: 5% to 6%, and water reducer: 0.1% to 0.2%.
[0011] As a further improvement of the present invention, the filler raw material components include, by weight percentage: fused quartz: 20% to 21%, calcined quartz: 20% to 23%, aluminum powder: 12% to 13%, iron powder: 12% to 13%, FeO: 9% to 11%, ZnO: 10% to 12%, CrN: 4% to 5%, active α-Al2O3: 5% to 6%, and water reducer: 0.1% to 0.2%.
[0012] The present invention provides a method for preparing the filler for the gap between coke oven wall bricks and steel plates, comprising the following steps:
[0013] 1) Weigh fused quartz, calcined quartz, aluminum powder, iron powder, FeO, ZnO, CrN, active α-Al2O3, and water reducer according to proportion, mix and stir to obtain a mixture;
[0014] 2) Add water to the mixed material, mix and stir to obtain a filler.
[0015] As a further improvement of the present invention, in step 1), the mixing and stirring are performed for 5 to 7 minutes.
[0016] As a further improvement of the present invention, in the step 2), 5% to 6% of water is added according to the total weight of the mixture.
[0017] As a further improvement of the present invention, in step 2), the mixing and stirring are performed for 8 to 10 minutes.
[0018] The present invention also provides a method for using a filler for repairing gaps between wall bricks and steel plates of a coke oven, comprising the following steps:
[0019] 1) The present invention uses fused quartz, calcined quartz, metal aluminum powder, metal iron powder, FeO, ZnO, and CrN as main materials, active α-Al2O3 powder as a binder, and sodium carbonate as a water reducer to prepare a filler. The filler of the present invention is directly injected into the gaps between the wall bricks and steel plates of the coke oven wall. The filler has good fluidity and can automatically fill the gaps;
[0020] 2) Wait until the filling material stops flowing before use.
[0021] The filler of the present invention meets the working requirements of the coke oven, and its main physical and chemical indicators are as follows: refractory temperature (℃): >1500, bulk density (g / cm 3 ): ≥2.5 (110℃×24h); ≥2.8 (1500℃×24h), compressive strength (MPa): ≥37 (110℃×24h); ≥52 (1500℃×24h), bonding strength (MPa): ≥28 (1500℃×24h), fluidity (mm): ≥280, line change after firing (%): ±0.1 (1500℃×24h).
[0022] Compared with the prior art, the advantages of the present invention are:
[0023] 1) The filler of the present invention can realize bidirectional melting and bonding with the furnace wall refractory bricks and steel plates, with high bonding strength and long hanging time.
[0024] 2) The filler of the present invention has good fluidity and can fill gaps without dead corners.
[0025] 3) The present invention utilizes self-propagating high temperature synthesis technology. The temperature of the coke oven itself will cause the metal aluminum powder and part of the iron powder to burn. The released heat allows the various phases of the filler to complete high-temperature sintering, and accompanied by the volume change of part of the raw materials, the gaps are filled completely and densely. DETAILED DESCRIPTION
[0026] The technical solution of the present invention is described in detail below in conjunction with embodiments.
[0027] The invention provides a filler for gaps between coke oven wall bricks and steel plates and a preparation method thereof. The filler contains, by weight percentage, 16-30% of fused quartz with a particle size of 3-5mm, 10-35% of calcined quartz with a particle size of 1-3mm, 10-15% of metal aluminum powder with a particle size of less than 30μm, 7-20% of metal iron powder with a particle size of less than 30μm, 5-20% of FeO with a particle size of 0.01-0.5mm, 5-15% of ZnO with a particle size of 0.01-1mm, 1-5% of CrN with a particle size of 0.01-1mm, 2-8% of active α-Al2O3 micro powder with a particle size of less than 0.088mm, and 0.1-0.3% of a water reducing agent. The filler has the advantages of high two-way bonding strength with refractory bricks and steel plates, long hanging time, good fluidity, solid filling of gaps, and the like.
[0028] The present invention also provides a method for preparing a filler for gaps between coke oven wall bricks and steel plates, comprising the following steps:
[0029] 1) Weigh various raw materials according to proportion, mix and stir for 5 to 7 minutes;
[0030] 2) Add 5% to 6% water of the total weight of the mixture, continue mixing and stirring for 8 to 10 minutes to obtain a filler.
[0031] Example 1
[0032] A new type of coke oven wall brick and steel plate gap filling material, the raw material formula of which is as follows:
[0033] In terms of weight percentage, the filler contains 30% of fused quartz with a particle size of 3 to 5 mm, 10% of calcined quartz with a particle size of 1 to 3 mm, 10% of metal aluminum powder with a particle size of less than 30 μm, 10% of metal iron powder with a particle size of less than 30 μm, 15% of FeO with a particle size of 0.01 to 0.5 mm, 15% of ZnO with a particle size of 0.01 to 1 mm, 5% of CrN with a particle size of 0.01 to 1 mm, 5% of active α-Al2O3 micropowder with a particle size of less than 0.088 mm, and 0.2% of sodium silicate.
[0034] Weigh various materials according to the proportions described in the raw material formula, put them into a blender and mix for 5 to 7 minutes; bag them for later use. Use fillers to repair the gaps between the furnace wall and the steel plate, add 5% to 6% of the total weight of the mixture into water, mix and stir for 8 to 10 minutes, then inject the fillers directly into the gaps between the coke oven wall bricks and the steel plate, and wait until the fillers stop flowing before use. Its main physical and chemical indicators are as follows: refractory temperature (℃) > 1500, volume density (g / cm 3)2.5(110℃×24h);2.9(1500℃×24h), compressive strength (MPa)38(110℃×24h);52(1500℃×24h), bonding strength (MPa)28(1500℃×24h), fluidity (mm)282, linear change after firing (%)±0.1(1500℃×24h).
[0035] Example 2
[0036] A new type of coke oven wall brick and steel plate gap filling material, the raw material formula of which is as follows:
[0037] In terms of weight percentage, the filler contains 22% of fused quartz with a particle size of 3 to 5 mm, 24% of calcined quartz with a particle size of 1 to 3 mm, 12% of metal aluminum powder with a particle size of less than 30 μm, 11% of metal iron powder with a particle size of less than 30 μm, 10% of FeO with a particle size of 0.01 to 0.5 mm, 12% of ZnO with a particle size of 0.01 to 1 mm, 3% of CrN with a particle size of 0.01 to 1 mm, 6% of active α-Al2O3 micropowder with a particle size of less than 0.088 mm, and 0.2% of sodium carbonate.
[0038] Weigh various materials according to the proportions described in the raw material formula, put them into a blender and mix for 5 to 7 minutes; bag them for later use. Use fillers to repair the gaps between the furnace wall and the steel plate, add 5% to 6% of the total weight of the mixture into water, mix and stir for 8 to 10 minutes, then inject the fillers directly into the gaps between the coke oven wall bricks and the steel plate, and wait until the fillers stop flowing before use. Its main physical and chemical indicators are as follows: refractory temperature (℃) > 1500, volume density (g / cm 3 )2.6(110℃×24h);2.8(1500℃×24h), compressive strength (MPa)38(110℃×24h);54(1500℃×24h), bonding strength (MPa)29(1500℃×24h), fluidity (mm)283, linear change after firing (%)±0.1(1500℃×24h).
[0039] Example 3
[0040] A new type of coke oven wall brick and steel plate gap filling material, the raw material formula of which is as follows:
[0041] In terms of weight percentage, the filler contains 23% fused quartz with a particle size of 3 to 5 mm, 22% calcined quartz with a particle size of 1 to 3 mm, 12% metal aluminum powder with a particle size of less than 30 μm, 12% metal iron powder with a particle size of less than 30 μm, 10% FeO with a particle size of 0.01 to 0.5 mm, 11% ZnO with a particle size of 0.01 to 1 mm, 4.5% CrN with a particle size of 0.01 to 1 mm, 5.5% active α-Al2O3 micropowder with a particle size of less than 0.088 mm, and 0.2% sodium carbonate.
[0042] Weigh various materials according to the proportions described in the raw material formula, put them into a blender and mix for 5 to 7 minutes; bag them for later use. Use fillers to repair the gaps between the furnace wall and the steel plate, add 5% to 6% of the total weight of the mixture into water, mix and stir for 8 to 10 minutes, then inject the fillers directly into the gaps between the coke oven wall bricks and the steel plate, and wait until the fillers stop flowing before use. Its main physical and chemical indicators are as follows: refractory temperature (℃) > 1500, volume density (g / cm 3 )2.5(110℃×24h);2.8(1500℃×24h), compressive strength (MPa)37(110℃×24h);53(1500℃×24h), bonding strength (MPa)29(1500℃×24h), fluidity (mm)280, linear change after firing (%)±0.1(1500℃×24h).
[0043] Example 4
[0044] A new type of coke oven wall brick and steel plate gap filling material, the raw material formula of which is as follows:
[0045] In terms of weight percentage, the filler contains 20% fused quartz with a particle size of 3 to 5 mm, 23% calcined quartz with a particle size of 1 to 3 mm, 13% metal aluminum powder with a particle size of less than 30 μm, 13% metal iron powder with a particle size of less than 30 μm, 11% FeO with a particle size of 0.01 to 0.5 mm, 11% ZnO with a particle size of 0.01 to 1 mm, 4% CrN with a particle size of 0.01 to 1 mm, 5% active α-Al2O3 micropowder with a particle size of less than 0.088 mm, and 0.2% sodium carbonate.
[0046] Weigh various materials according to the proportions described in the raw material formula, put them into a blender and mix for 5 to 7 minutes; bag them for later use. Use fillers to repair the gaps between the furnace wall and the steel plate, add 5% to 6% of the total weight of the mixture into water, mix and stir for 8 to 10 minutes, then inject the fillers directly into the gaps between the coke oven wall bricks and the steel plate, and wait until the fillers stop flowing before use. Its main physical and chemical indicators are as follows: refractory temperature (℃) > 1500, volume density (g / cm 3)2.6(110℃×24h);2.8(1500℃×24h), compressive strength (MPa)37(110℃×24h);53(1500℃×24h), bonding strength (MPa)28(1500℃×24h), fluidity (mm)281, linear change after firing (%)±0.1(1500℃×24h).
[0047] Example 5
[0048] A new type of coke oven wall brick and steel plate gap filling material, the raw material formula of which is as follows:
[0049] In terms of weight percentage, the filler contains 22% of fused quartz with a particle size of 3 to 5 mm, 20% of calcined quartz with a particle size of 1 to 3 mm, 15% of metal aluminum powder with a particle size of less than 30 μm, 14% of metal iron powder with a particle size of less than 30 μm, 6% of FeO with a particle size of 0.01 to 0.5 mm, 15% of ZnO with a particle size of 0.01 to 1 mm, 5% of CrN with a particle size of 0.01 to 1 mm, 3% of active α-Al2O3 micropowder with a particle size of less than 0.088 mm, and 0.2% of sodium carbonate.
[0050] Weigh various materials according to the proportions described in the raw material formula, put them into a blender and mix for 5 to 7 minutes; bag them for later use. Use fillers to repair the gaps between the furnace wall and the steel plate, add 5% to 6% of the total weight of the mixture into water, mix and stir for 8 to 10 minutes, then inject the fillers directly into the gaps between the coke oven wall bricks and the steel plate, and wait until the fillers stop flowing before use. Its main physical and chemical indicators are as follows: refractory temperature (℃) > 1500, volume density (g / cm 3 )2.5 (110℃×24h); 3.0 (1500℃×24h), compressive strength (MPa) 39 (110℃×24h); 53 (1500℃×24h), bonding strength (MPa) 29 (1500℃×24h), fluidity (mm) 282, linear change after firing (%) ±0.1 (1500℃×24h).
[0051] Example 6
[0052] A new type of coke oven wall brick and steel plate gap filling material, the raw material formula of which is as follows:
[0053] In terms of weight percentage, the filler contains 19% of fused quartz with a particle size of 3 to 5 mm, 21% of calcined quartz with a particle size of 1 to 3 mm, 13% of metal aluminum powder with a particle size of less than 30 μm, 12% of metal iron powder with a particle size of less than 30 μm, 16% of FeO with a particle size of 0.01 to 0.5 mm, 10% of ZnO with a particle size of 0.01 to 1 mm, 2% of CrN with a particle size of 0.01 to 1 mm, 7% of active α-Al2O3 micropowder with a particle size of less than 0.088 mm, and 0.2% of sodium carbonate.
[0054] Weigh various materials according to the proportions described in the raw material formula, put them into a blender and mix for 5 to 7 minutes; bag them for later use. Use fillers to repair the gaps between the furnace wall and the steel plate, add 5% to 6% of the total weight of the mixture into water, mix and stir for 8 to 10 minutes, then inject the fillers directly into the gaps between the coke oven wall bricks and the steel plate, and wait until the fillers stop flowing before use. Its main physical and chemical indicators are as follows: refractory temperature (℃) > 1500, volume density (g / cm 3 )2.5(110℃×24h);2.9(1500℃×24h), compressive strength (MPa)37(110℃×24h);52(1500℃×24h), bonding strength (MPa)30(1500℃×24h), fluidity (mm)280, linear change after firing (%)±0.1(1500℃×24h).
[0055] Example 7
[0056] A new type of coke oven wall brick and steel plate gap filling material, the raw material formula of which is as follows:
[0057] In terms of weight percentage, the filler contains 21% of fused quartz with a particle size of 3 to 5 mm, 31% of calcined quartz with a particle size of 1 to 3 mm, 10% of metal aluminum powder with a particle size of less than 30 μm, 13% of metal iron powder with a particle size of less than 30 μm, 12% of FeO with a particle size of 0.01 to 0.5 mm, 8% of ZnO with a particle size of 0.01 to 1 mm, 1% of CrN with a particle size of 0.01 to 1 mm, 4% of active α-Al2O3 micropowder with a particle size of less than 0.088 mm, and 0.2% of sodium carbonate.
[0058] Weigh various materials according to the proportions described in the raw material formula, put them into a blender and mix for 5 to 7 minutes; bag them for later use. Use fillers to repair the gaps between the furnace wall and the steel plate, add 5% to 6% of the total weight of the mixture into water, mix and stir for 8 to 10 minutes, then inject the fillers directly into the gaps between the coke oven wall bricks and the steel plate, and wait until the fillers stop flowing before use. Its main physical and chemical indicators are as follows: refractory temperature (℃) > 1500, volume density (g / cm 3)2.6(110℃×24h);2.9(1500℃×24h), compressive strength (MPa)38(110℃×24h);53(1500℃×24h), bonding strength (MPa)28(1500℃×24h), fluidity (mm)281, linear change after firing (%)±0.1(1500℃×24h).
[0059] The process parameters (such as temperature, time, etc.) of the present invention can realize the method by taking upper and lower limits and interval values, and the embodiments are not listed one by one here.
[0060] Any contents not described in detail in the present invention can be based on the conventional technical knowledge in the art.
[0061] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention is described in detail with reference to the embodiments, it should be understood by those skilled in the art that any modification or equivalent replacement of the technical solutions of the present invention does not depart from the spirit and scope of the technical solutions of the present invention and should be included in the scope of the claims of the present invention.
Claims
1. A filler for the gap between coke oven wall bricks and steel plates. It is characterized in that The filler raw material components include, by weight percentage: fused quartz: 16% to 30%, calcined quartz: 10% to 35%, aluminum powder: 10% to 15%, iron powder: 7% to 20%, FeO: 5% to 20%, ZnO: 5% to 15%, CrN: 1% to 5%, active α-Al 2 O 3 : 2%~8%, water reducing agent: 0.1%~0.3%.
2. The filler for the gap between coke oven wall bricks and steel plates according to claim 1, It is characterized in that The particle size distribution of the fused quartz is 3mm to 5mm, the particle size distribution of the calcined quartz is 1mm to 3mm, the particle size distribution of the aluminum powder is less than 30μm and is not equal to 0mm, the particle size distribution of the iron powder is less than 30μm and is not equal to 0mm, the particle size distribution of FeO is 0mm to 0.5mm and is not equal to 0mm, the particle size distribution of ZnO is 0mm to 1mm and is not equal to 0mm, the particle size distribution of CrN is 0mm to 1mm and is not equal to 0mm, and the active α-Al 2 O 3 The particle size distribution is less than 0.088mm, and the particle size distribution of the water reducer is 175-185 mesh.
3. The filler for the gap between coke oven wall bricks and steel plates according to claim 1, It is characterized in that The water reducing agent is sodium carbonate.
4. The filler for the gap between coke oven wall bricks and steel plates according to any one of claims 1 to 3, It is characterized in that The filler raw material components include, by weight percentage: fused quartz: 17% to 26%, calcined quartz: 15% to 31%, aluminum powder: 12% to 14%, iron powder: 9% to 15%, FeO: 5% to 15%, ZnO: 7% to 13%, CrN: 3% to 5%, active α-Al 2 O 3 : 4%~7%, water reducing agent: 0.1%~0.2%.
5. The filler for the gap between coke oven wall bricks and steel plates according to any one of claims 1 to 3, It is characterized in that The filler raw material components include, by weight percentage: fused quartz: 19% to 22%, calcined quartz: 19% to 25%, aluminum powder: 12% to 13%, iron powder: 11% to 13%, FeO: 7% to 12%, ZnO: 8% to 12%, CrN: 4% to 5%, active α-Al 2 O 3 : 5%~6%, water reducing agent: 0.1%~0.2%.
6. The filler for the gap between coke oven wall bricks and steel plates according to any one of claims 1 to 3, It is characterized in that The filler raw material components include, by weight percentage: fused quartz: 20% to 21%, calcined quartz: 20% to 23%, aluminum powder: 12% to 13%, iron powder: 12% to 13%, FeO: 9% to 11%, ZnO: 10% to 12%, CrN: 4% to 5%, active α-Al 2 O 3 : 5%~6%, water reducing agent: 0.1%~0.2%.
7. A method for preparing the filler for gaps between coke oven wall bricks and steel plates as claimed in any one of claims 1 to 6, The following steps are involved: 1) Weigh fused quartz, calcined quartz, aluminum powder, iron powder, FeO, ZnO, CrN, active α-Al 2 O 3 , a water reducing agent, and mixing and stirring to obtain a mixture; 2) Add water to the mixed material, mix and stir to obtain a filler.
8. The method for preparing the filler for the gap between coke oven wall bricks and steel plates according to claim 7, It is characterized in that In the step 1), the mixture is mixed and stirred for 5 to 7 minutes.
9. The method for preparing the filler for the gap between coke oven wall bricks and steel plates according to claim 7, It is characterized in that In the step 2), 5% to 6% of water is added according to the total weight of the mixture.
10. The method for preparing the filler for the gap between coke oven wall bricks and steel plates according to claim 7, It is characterized in that In the step 2), the mixture is mixed and stirred for 8 to 10 minutes.
Citation Information
Patent Citations
RH insert tube scalding material and RH insert tube scalding method
CN104193360A
Heating and heat-insulating filling liner
CN106699198A
Coke oven ceramic hot smearing supplementary material and preparation method thereof
CN108276010A
Preparation method of self-flowing type hot-state repairing material for coke oven coke tank
CN113354429A
Thermal shock resistant silica brick for hot repairing and its production
JP2000327408A