Honeycomb structure manufacturing method and honeycomb structure

By combining cross-linked starch and acrylic polymer in the honeycomb structure, and adjusting their ratio and content, the problem of insufficient strength during the process of thinning and high porosity is solved, and efficient manufacturing of honeycomb structures is achieved to meet the needs of High capture performance and low heat capacity requirements.

CN118724607AActive Publication Date: 2024-10-01NGK INSULATORS LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410308093.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-18
Publication Date
2024-10-01
Estimated Expiration
2044-03-18

AI Technical Summary

Technical Problem

During the process of thinning the walls and increasing the porosity of existing honeycomb structures, the strength is insufficient, and the extrusion molding pressure is too high, which increases the burden on the molding machine and makes it difficult to meet the requirements of high capture performance and low heat capacity.

Method used

Cross-linked starch and acrylic polymer are used as pore-forming materials. By adjusting their proportion and content, the extrusion molding pressure is reduced and the porosity and strength of the honeycomb structure are increased.

Benefits of technology

It is possible to produce a honeycomb structure with excellent strength and high porosity without increasing the burden on the extrusion molding machine. It is suitable as a high-efficiency filter and catalyst carrier to meet the needs of high collection performance and rapid temperature rise.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724607A_ABST
    Figure CN118724607A_ABST
Patent Text Reader

Abstract

The invention provides a manufacturing method of a honeycomb structure and the honeycomb structure. The manufacturing method comprises the following steps: a step of preparing a honeycomb molded body by extruding and molding blank soil; a step of drying to obtain a honeycomb dried body; and a step of firing to obtain a honeycomb fired body with a partition wall thickness of 50-210 [mu] m and a partition wall porosity of 45-60%. The pore-forming material in the clay contains a crosslinked starch and an acrylic polymer, and the clay contains 1.0 parts by mass or more of the crosslinked starch under the condition that the P content is less than 0.2 parts by mass with respect to 100 parts by mass of the ceramic raw material. The honeycomb structure has an outer peripheral side wall and partition walls, the partition walls are disposed on the inner peripheral side of the outer peripheral side wall and define a plurality of cells, the thickness of the partition walls is 50 [mu] m-210 [mu] m, the porosity is 45%-60%, the P content in the honeycomb structure is 0.01 mass% or more and less than 0.2 mass%, and the isostatic pressing breaking strength is 1.0 MPa or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a honeycomb structure and the honeycomb structure. Background Art

[0002] Honeycomb structures are used as filters for collecting particulate matter in exhaust gas discharged from internal combustion engines such as diesel engines, and as catalyst carriers for purifying poisonous gas components such as CO, HC, and NOx.

[0003] Generally, a honeycomb structure has an outer peripheral side wall and a partition wall, which is arranged on the inner peripheral side of the outer peripheral side wall and divides a plurality of cells that form a flow path from the first bottom surface to the second bottom surface. The honeycomb structure can be manufactured as follows: a raw material composition obtained by appropriately adding various additives to a ceramic raw material, a pore-forming material, a binder, and a dispersion medium is kneaded to form a green clay, and then extruded through a die defining a predetermined cell structure to produce a honeycomb molded body, and the honeycomb molded body is cut into a predetermined length, dried, and then fired.

[0004] In recent years, with the strengthening of exhaust gas restrictions, stricter PM emission standards (PN restrictions: Particle Matter number restrictions) have been introduced, and filters are required to have high PM capture performance (PN high capture efficiency). In addition, the catalyst carrier is also required to be able to quickly heat up to the active temperature of the catalyst by reducing the heat capacity. On the other hand, the honeycomb structure is also required to have a low pressure loss when exhaust gas flows in, and the difficulty of developing filters that can meet market requirements has increased. In order to obtain a honeycomb structure that meets such required performance, research has been conducted on "thinning" to thin the thickness of the partition walls of the honeycomb structure, and "high porosity" to further increase the porosity of the partition walls compared to the past (Patent Document 1).

[0005] However, with the progress of thin-walled honeycomb structures, the extrusion molding pressure required to extrude the green clay through an extremely narrow die groove has also increased, reaching the limit of the extruder. Therefore, a technology for reducing the extrusion molding pressure is also required. In connection with this, in Patent Document 2, it is recorded that if the amylose ratio in the starch added to the raw material composition is high, the fluidity becomes better and the molding pressure decreases, and in particular, it is disclosed that the extrusion molding pressure can be reduced when the ratio of amylose: amylopectin is 40:60 to 80:20.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application No. 2007-507667

[0009] Patent Document 2: International Publication No. 2017 / 095916 Summary of the invention

[0010] Problems to be solved by the invention

[0011] Starch is useful as a component for obtaining a honeycomb structure with high porosity. Therefore, it is believed that when manufacturing a honeycomb structure with thin walls and high porosity, it is effective to add starch in the proportion of amylose and amylopectin described in Patent Document 2. However, even if the extrusion molding pressure can be reduced by adding starch in which the proportion of amylose and amylopectin is adjusted in this way to the raw material composition, the strength of the honeycomb structure manufactured thereby is insufficient. In particular, the strength of a honeycomb structure with thin walls and high porosity is easily reduced, so it would be advantageous if this problem could be solved.

[0012] The present invention is completed in view of the above situation, and the subject of one embodiment is to provide a method for manufacturing a thin-walled, high-porosity, and excellent-strength honeycomb structure without placing an excessive burden on an extruder. In addition, the subject of another embodiment is to provide a thin-walled, high-porosity, and excellent-strength honeycomb structure.

[0013] Methods for solving problems

[0014] The present inventors have conducted intensive studies to solve the above problems and have found that it is effective to use an acrylic acid-based polymer and a cross-linked starch in combination as a pore-forming material. The present invention has been completed based on this finding and is exemplified below.

[0015] (1. Method for manufacturing honeycomb structure)

[0016] [Method 1]

[0017] A method for manufacturing a honeycomb structure, the honeycomb structure having an outer peripheral side wall and partition walls, the partition walls being arranged on the inner peripheral side of the outer peripheral side wall and dividing a plurality of cells forming a flow path from a first bottom surface to a second bottom surface, the manufacturing method being characterized in that it comprises: a step of extruding a molded body containing a ceramic raw material, a pore-forming material, an adhesive and a dispersion medium through a die having an opening shape defining the plurality of cells, thereby manufacturing a honeycomb formed body, a step of drying the honeycomb formed body to obtain a honeycomb dried body, and a step of firing the honeycomb dried body to obtain a honeycomb fired body having a partition wall thickness of not less than 50 μm and not more than 210 μm and a partition wall porosity of 45% to 60%; the pore-forming material in the molded body contains cross-linked starch and an acrylic polymer, and the molded body contains more than 1.0 mass part of cross-linked starch relative to 100 mass parts of the ceramic raw material under the condition that the P content becomes less than 0.2 mass part.

[0018] [Method 2]

[0019] The production method according to aspect 1, wherein the kneaded clay contains 1.0 part by mass or more of cross-linked starch based on 100 parts by mass of the ceramic raw material under the condition that the P content is 0.1 part by mass or less.

[0020] [Method 3]

[0021] The production method according to aspect 1, wherein the kneaded clay contains 1.0 part by mass or more of cross-linked starch based on 100 parts by mass of the ceramic raw material under the condition that the P content is 0.05 parts by mass or less.

[0022] [Method 4]

[0023] The production method according to any one of aspects 1 to 3, wherein a P content in the honeycomb structure is less than 0.2 mass %.

[0024] [Method 5]

[0025] The production method according to any one of aspects 1 to 3, wherein a P content in the honeycomb structure is 0.1 mass % or less.

[0026] [Method 6]

[0027] The production method according to any one of aspects 1 to 3, wherein a P content in the honeycomb structure is 0.05 mass % or less.

[0028] [Method 7]

[0029] The production method according to any one of aspects 1 to 6, wherein the kneaded clay contains 0.5 parts by mass or more of the acrylic polymer based on 100 parts by mass of the ceramic raw material.

[0030] [Method 8]

[0031] The production method according to any one of aspects 1 to 7, wherein the ceramic raw material is a cordierite forming raw material.

[0032] (2. Honeycomb structure)

[0033] [Method 1]

[0034] A honeycomb structure having an outer peripheral side wall and partition walls, wherein the partition walls are arranged on the inner peripheral side of the outer peripheral side wall and divide a plurality of cells that form a flow path from a first bottom surface to a second bottom surface, the thickness of the partition walls is greater than 50 μm and less than 210 μm, the porosity of the partition walls is 45% to 60%, the P content in the honeycomb structure is greater than 0.01 mass % and less than 0.2 mass %, and the isostatic pressure fracture strength is greater than 1.0 MPa.

[0035] [Method 2]

[0036] The honeycomb structure according to Embodiment 1, wherein an upper limit of a P content in the honeycomb structure is 0.1 mass % or less.

[0037] [Method 3]

[0038] The honeycomb structure according to Embodiment 1, wherein an upper limit of a P content in the honeycomb structure is 0.05 mass % or less.

[0039] [Method 4]

[0040] The honeycomb structure according to any one of aspects 1 to 3, wherein the outer peripheral side walls and the partition walls contain cordierite.

[0041] Effects of the Invention

[0042] According to one embodiment of the present invention, a thin-walled, high-porosity, and strong honeycomb structure can be manufactured with high productivity without placing excessive burden on an extruder. The honeycomb structure can be used as a filter or a catalyst carrier, and is particularly useful as a filter requiring high capture performance (PN high capture efficiency) or a catalyst carrier requiring a high heating rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 It is a perspective view schematically showing a wall-through type honeycomb structure.

[0044] Figure 2 This is a schematic cross-sectional view of a wall-through type honeycomb structure observed in a cross section parallel to the direction in which cells extend.

[0045] Figure 3 It is a perspective view schematically showing a wall-flow type honeycomb structure.

[0046] Figure 4 This is a schematic cross-sectional view of a wall flow type honeycomb structure observed in a cross section parallel to the direction in which cells extend.

[0047] Figure 5 This is a schematic partial enlarged view when observing the partition wall of the wall flow type honeycomb structure in a cross section perpendicular to the cell extending direction.

[0048] Description of Reference Numerals

[0049] 100: honeycomb structure, 102: outer peripheral side wall, 103: side surface, 104: first bottom surface, 106: second bottom surface, 108: cells, 112: partition walls, 200: honeycomb structure, 202: outer peripheral side wall, 203: side surface, 204: first bottom surface, 206: second bottom surface, 208a: first cells, 208b: second cells, 209: sealing portion, 212: partition walls. DETAILED DESCRIPTION

[0050] Next, embodiments of the present invention will be described in detail with reference to the accompanying drawings. It should be understood that the present invention is not limited to the following embodiments, and design changes and improvements may be appropriately applied based on the common knowledge of those skilled in the art without departing from the gist of the present invention.

[0051] <1. Honeycomb structure>

[0052] In one embodiment, the honeycomb structure of the present invention is provided as a wall-penetrating or wall-flow type honeycomb structure. The use of the honeycomb structure is not particularly limited. For example, it can be used for various industrial uses such as radiators, filters (e.g., GPF, DPF), catalyst carriers, sliding parts, nozzles, heat exchangers, electrical insulation parts, and semiconductor manufacturing equipment parts. Among them, it can be suitable for use as a filter for capturing particulate matter contained in exhaust gas from internal combustion engines, boilers, etc., and a catalyst carrier for exhaust gas purification catalyst. In particular, the porous honeycomb structure can be suitable for use as an automotive exhaust gas filter and / or catalyst carrier.

[0053] exist Figure 1 and Figure 2 , schematic stereograms and cross-sectional diagrams of a honeycomb structure 100 that can be used as a wall-penetrating automobile exhaust gas filter and / or catalyst carrier are respectively illustrated. The honeycomb structure 100 includes an outer peripheral side wall 102 and a partition wall 112, the partition wall 112 being arranged on the inner peripheral side of the outer peripheral side wall 102 and dividing a plurality of parallel cells 108 that form a fluid flow path from a first bottom surface 104 to a second bottom surface 106. The outer surface of the outer peripheral side wall 102 forms a side surface 103 of the honeycomb structure 100. In the honeycomb structure 100, both ends of each cell 108 are open, and the exhaust gas flowing into one cell 108 from the first bottom surface 104 is purified in the process of passing through the cell and flows out from the second bottom surface 106. It should be noted that, here, the first bottom surface 104 is set as the upstream side of the exhaust gas, and the second bottom surface 106 is set as the downstream side of the exhaust gas, but the distinction between the first bottom surface and the second bottom surface is for convenience, and the second bottom surface 106 can also be set as the upstream side of the exhaust gas, and the first bottom surface 104 can be set as the downstream side of the exhaust gas.

[0054] exist Figure 3 and Figure 4, a schematic perspective view and a cross-sectional view of a honeycomb structure 200 that can be used as a wall-flow type automobile exhaust gas filter and / or catalyst carrier are respectively illustrated. The honeycomb structure 200 includes an outer peripheral side wall 202 and a partition wall 212, the partition wall 212 being arranged on the inner peripheral side of the outer peripheral side wall 202 and dividing a plurality of cells 208a, 208b that form a fluid flow path from a first bottom surface 204 to a second bottom surface 206. The outer surface of the outer peripheral side wall 202 forms a side surface 203 of the honeycomb structure 200.

[0055] In the honeycomb structure 200, the plurality of cells 208a and 208b can be classified into: a plurality of parallel first cells 208a extending from the first bottom surface 204 to the second bottom surface 206, opening on the first bottom surface 204 and having a plugging portion 209 on the second bottom surface 206; and a plurality of parallel second cells 208b arranged on the inner side of the outer peripheral side wall 202, extending from the first bottom surface 204 to the second bottom surface 206, having a plugging portion 209 on the first bottom surface 204 and opening on the second bottom surface 206. In addition, in the honeycomb structure 200, the first cells 208a and the second cells 208b are alternately arranged adjacent to each other with the partition wall 212 interposed therebetween.

[0056] When exhaust gas containing particulate matter such as soot is supplied to the first bottom surface 204 on the upstream side of the honeycomb structure 200, the exhaust gas is introduced into the first cell 208a and moves downstream in the first cell 208a. Since the first cell 208a has a sealing portion 209 on the second bottom surface 206 on the downstream side, the exhaust gas flows into the second cell 208b through the partition 212 that divides the first cell 208a and the second cell 208b. Since the particulate matter cannot pass through the partition 212, it is captured and accumulated in the first cell 208a. After the particulate matter is removed, the clean exhaust gas that has flowed into the second cell 208b moves downstream in the second cell 208b and flows out from the second bottom surface 206 on the downstream side. It should be noted that, here, the first bottom surface 204 is set as the upstream side of the exhaust gas, and the second bottom surface 206 is set as the downstream side of the exhaust gas, but the distinction between the first bottom surface and the second bottom surface is for convenience, and the second bottom surface 206 can also be set as the upstream side of the exhaust gas, and the first bottom surface 204 can be set as the downstream side of the exhaust gas.

[0057] The shape of the honeycomb structure can be, for example, a column. The bottom shape of the honeycomb structure is not limited, and can be, for example, a circular, elliptical, racetrack-shaped, oblong, or other curved shapes, a triangular, quadrilateral, or other polygonal shapes, and other special shapes. The bottom shape of the illustrated honeycomb structure is circular, and the whole is cylindrical.

[0058] The height of the honeycomb structure (the length from the first bottom surface to the second bottom surface) is not particularly limited and can be appropriately set according to the application and required performance. The height of the honeycomb structure can be set to 40 mm to 450 mm, for example. There is no particular restriction on the relationship between the height of the honeycomb structure and the maximum diameter of each bottom surface (referring to the maximum length of the diameter of the center of gravity of each bottom surface of the honeycomb structure). Therefore, the height of the honeycomb structure can be longer than the maximum diameter of each bottom surface, and the height of the honeycomb structure can also be shorter than the maximum diameter of each bottom surface.

[0059] The cell density (the number of cells per unit cross-sectional area perpendicular to the direction in which the cells extend) of the honeycomb structure is not particularly limited, and can be, for example, 6 to 2000 cells / square inch (0.9 to 311 cells / cm 2 ), and more preferably 50 to 1000 cells / square inch (7.8 to 155 cells / cm 2 ), particularly preferably 100 to 600 cells / square inch (15.5 to 92.0 cells / cm 2 Here, the cell density is calculated by dividing the total number of cells in the bottom surface (when there are plugged cells, the cells are calculated as unplugged cells) by the bottom area of ​​the honeycomb structure excluding the peripheral side wall.

[0060] From the viewpoint of reducing the pressure loss and lowering the heat capacity by thinning the wall, the thickness of the partition wall in the honeycomb structure is preferably 210 μm or less, more preferably 150 μm or less, and further preferably 100 μm or less. In addition, from the viewpoint of ensuring strength, the thickness of the partition wall in the honeycomb structure is preferably 50 μm or more, more preferably 60 μm or more, and further preferably 70 μm or more.

[0061] Figure 5 2 shows a schematic partial enlarged view of a partition wall 212 of a wall-flow type honeycomb structure 200 observed in a cross section perpendicular to the direction in which the cells extend. The thickness of the partition wall refers to the length of the line segment N that crosses the partition wall when the centroids C of adjacent cells are connected to each other in the cross section perpendicular to the direction in which the cells extend (the height direction of the honeycomb structure).

[0062] From the viewpoint of suppressing pressure loss and reducing heat capacity by increasing porosity, the porosity of the partition wall is preferably 45% or more, and more preferably 50% or more. In addition, from the viewpoint of ensuring the strength of the thin-walled honeycomb structure, the upper limit of the porosity of the partition wall is preferably 60% or less, and more preferably 55% or less. Therefore, the porosity of the partition wall is preferably, for example, 45% to 60%, and more preferably 50% to 55%. The porosity is measured by mercury intrusion using a mercury porosimeter. The mercury intrusion method is specified in JIS R1655:2003. In this specification, partition wall samples of the honeycomb structure (cubes with a length × width × height = about 13 mm × about 13 mm × about 13 mm) are taken from two locations near the radial center of the center in the height direction and near the periphery, and the porosity is measured by mercury intrusion, and the average value is taken as the measured value.

[0063] As the material constituting the partition wall and the peripheral side wall of the honeycomb structure, there is no limitation, and porous ceramics can be cited. As the type of ceramics, cordierite, mullite, zirconium phosphate, aluminum titanate, silicon carbide (SiC), silicon-silicon carbide composite materials (example: Si combined with SiC), cordierite-silicon carbide composite materials, zirconium oxide, spinel, India stone, pseudo sapphire, corundum, titanium dioxide, silicon nitride, etc. can be cited. And, these ceramics can contain one alone, and can also contain more than two.

[0064] From the perspective of high heat shock resistance, the partition walls and peripheral side walls of the honeycomb structure preferably contain cordierite. The mass proportion of cordierite in the honeycomb structure is preferably 50 mass% or more, preferably 70 mass% or more, and preferably 90 mass% or more. In the porous honeycomb structure containing cordierite, the mass proportion of cordierite can also be substantially 100 mass% excluding unavoidable impurities.

[0065] In the honeycomb structure, the raw materials mixed in the raw material composition may remain. As described later, a cross-linking agent containing P (phosphorus) is sometimes used in the cross-linked starch, but if the cross-linking agent containing P is large, agglomerates will be generated in the green clay, which easily leads to an increase in the extrusion molding pressure. Therefore, when the P content in the cross-linked starch used as the pore-forming material is small, the extrusion molding pressure can be reduced, and the residual P concentration in the honeycomb structure is also low.

[0066] Therefore, in one embodiment, the P content in the honeycomb structure is less than 0.2% by mass, preferably less than 0.1% by mass, and more preferably less than 0.05% by mass. From the viewpoint of improving the effect of reducing the extrusion molding pressure, the P content in the honeycomb structure can be less than 0.01% by mass, and can further be 0, but the starch cross-linked with a cross-linking agent containing P has a high effect of suppressing cell deformation during extrusion molding, resulting in a high effect of improving the strength of the honeycomb structure. Therefore, from the balance with the effect of reducing the extrusion molding pressure, the P content in the honeycomb structure is preferably 0.01% by mass or more and less than 0.2% by mass, and more preferably 0.01% by mass or more and 0.05% by mass or less.

[0067] The P content in the honeycomb structure is determined by the following method. First, a partition wall sample (0.5 to 5.0 g) is collected from two locations near the radial center and the periphery of the central part in the height direction of the honeycomb structure. Sulfuric acid is added to each partition wall sample and heated. After ashing, it is dissolved in hydrochloric acid to prepare a sample solution. The sample solution is sprayed into a high-temperature argon plasma generated by high-frequency energy, and the emission intensity of the characteristic wavelength of the excited P atoms is measured using a sequential inductively coupled plasma emission spectrometer (ICP-OES / AES), and converted into the P content in the honeycomb structure. The average value of the P content in the honeycomb structure obtained from each partition wall sample is taken as the measured value.

[0068] One standard of the mechanical strength of a honeycomb structure is the isostatic breaking strength. In the determination of the isostatic breaking strength of a honeycomb structure, the following test is performed: the honeycomb structure is sunk into water in a pressure vessel, and the water pressure is gradually increased, thereby applying isotropic pressure to the honeycomb structure. As the water pressure in the pressure vessel gradually increases, damage eventually occurs to the partition walls and peripheral side walls of the honeycomb structure. The value of the pressure when damage occurs (destructive strength) is the isostatic breaking strength. The isostatic breaking strength is measured based on the automotive standard (JASO M505-87) issued by the Association of Automotive Engineers.

[0069] In one embodiment, even if the honeycomb structure is thin-walled and high-porosity, it can have an isostatic fracture strength of 1.0 MPa or more. The isostatic fracture strength of the honeycomb structure is preferably 1.5 MPa or more, more preferably 2.0 MPa or more. The upper limit of the isostatic fracture strength is not particularly set, but is usually 3.0 MPa or less, typically 2.5 MPa or less.

[0070] When the honeycomb structure is used as a catalyst carrier, a catalyst corresponding to the purpose can be coated on the surface of the partition wall. The catalyst can be used alone or in combination of two or more. As the catalyst, there is no limitation, and examples include an oxidation catalyst (DOC) for oxidizing and burning hydrocarbons (HC) and carbon monoxide (CO) to increase the exhaust gas temperature, a PM combustion catalyst for assisting the combustion of PM such as soot, an SCR catalyst and an NSR catalyst for removing nitrogen oxides (NOx), and a three-way catalyst that can simultaneously remove hydrocarbons (HC), carbon monoxide (CO) and nitrogen oxides (NOx). The catalyst can, for example, appropriately contain precious metals (Pt, Pd, Rh, etc.), alkali metals (Li, Na, K, Cs, etc.), alkaline earth metals (Mg, Ca, Ba, Sr, etc.), rare earths (Ce, Sm, Gd, Nd, Y, La, Pr, etc.), transition metals (Mn, Fe, Co, Ni, Cu, Zn, Sc, Ti, Zr, V, Cr, etc.), etc.

[0071] <2. Method for manufacturing honeycomb structure>

[0072] A method for producing a honeycomb structure according to one embodiment of the present invention will be described below by way of example.

[0073] (2-1. Preparation of Honeycomb Molded Body)

[0074] First, after kneading a raw material composition containing a ceramic raw material, a pore-forming material, an adhesive and a dispersion medium to form a green clay, the green clay is extruded through a die defining the opening shape of a plurality of cells, thereby making a honeycomb formed body having a peripheral side wall, and an inner peripheral side arranged on the peripheral side wall, extending from the first bottom surface to the second bottom surface and having a plurality of cells with openings on both the first bottom surface and the second bottom surface. Additives such as dispersants can be added to the raw material composition as needed. During extrusion molding, a die having a desired overall shape, cell shape, wall thickness, cell density, etc. can be used.

[0075] The ceramic raw material remains after firing, and is the raw material of the part of the skeleton that constitutes the honeycomb structure as ceramic. As the ceramic raw material, a raw material that can form the above-mentioned ceramic after firing can be used. The ceramic raw material can be provided in the form of a powder, for example. As the ceramic raw material, cordierite, mullite, zircon, aluminum titanate, silicon carbide, silicon nitride, zirconium oxide, spinel, India stone, sapphire, corundum, titanium dioxide and the like are raw materials for obtaining ceramics. Specifically, there is no limitation, and silicon dioxide, talc, aluminum oxide, kaolin, serpentine, pyrophyllite, brucite, boehmite, mullite, magnesite, aluminum hydroxide and the like can be cited. One ceramic raw material can be used alone, or two or more can be used in combination.

[0076] As a ceramic, cordierite can be used appropriately. At this time, as a ceramic raw material, a cordierite raw material can be used. The cordierite raw material refers to a raw material that becomes cordierite by firing. As a cordierite raw material, talc, kaolin, alumina, aluminum hydroxide, silicon dioxide, etc. can be used. The cordierite raw material is preferably composed of a chemical composition of 30 to 45% by mass of aluminum oxide (Al2O3) (including aluminum hydroxide converted into alumina) 11 to 17% by mass, and 42 to 57% by mass of silicon dioxide (SiO2).

[0077] Including cordierite raw materials, ceramic raw materials affect the strength of the honeycomb structure, so it is preferred to use raw materials whose particle size has been adjusted by crushing, screening, etc. Specifically, in the volume-based cumulative particle size distribution measured by the laser diffraction scattering method, the lower limit of the cumulative 50% particle size (D50) of each ceramic raw material from the small particle side is preferably 0.1μm or more, more preferably 0.5μm or more, and further preferably 1.0μm or more. In addition, the upper limit of the cumulative 50% particle size (D50) of each ceramic raw material from the small particle side is preferably 30μm or less, more preferably 20μm or less, and further preferably 15μm or less. Therefore, for example, the cumulative 50% particle size (D50) of each ceramic raw material is preferably 0.1μm or more and 30μm or less, more preferably 0.5μm or more and 20μm or less, and further preferably 1.0μm or more and 15μm or less.

[0078] As a pore-forming material, if cross-linked starch and acrylic polymer are used in combination, the fluidity of the green clay is significantly improved. As a result, the moldability is optimized, and the cellular deformation that is easily produced during molding is suppressed. Therefore, as a result, the strength of the honeycomb structure can be improved. In order to make the honeycomb structure thin-walled, it is necessary to extrude the green clay through an extremely narrow die groove, and the extrusion molding pressure also increases, which easily produces deformation of the cellular shape (cellular deformation). The reason why the cellular deformation can be suppressed by using cross-linked starch and acrylic polymer as pore-forming materials may not be clear. The present invention is not intended to be limited by theory, but it can be inferred that the water retention effect of cross-linked starch and acrylic polymer is related to the optimization of moldability. Compared with the case of using only either cross-linked starch or acrylic polymer, a significant effect can be obtained when the two are used together.

[0079] In cross-linked starch, one or more cross-linking agents such as formalin, epichlorohydrin and phosphate are used, so that several hydroxyl groups between starch molecules are cross-linked. Examples of cross-linked starch include acetylated adipic acid cross-linked starch, acetylated phosphate cross-linked starch, hydroxypropylated phosphate cross-linked starch, phosphate monoesterified phosphate cross-linked starch and phosphate cross-linked starch. One type of cross-linked starch may be used alone, or two or more types may be used in combination.

[0080] Thus, the cross-linked starch sometimes contains phosphorus (P). In addition, from the viewpoint of achieving a high porosity while obtaining the effect of improving the strength of the honeycomb structure, a cross-linked starch containing P is preferred. However, if the P content in the cross-linked starch increases, the screen used for removing impurities during the extrusion molding of the green clay is clogged, which becomes a cause of the increase in the extrusion molding pressure, so it is preferred to control the P content in the green clay within a range where the screen is not clogged.

[0081] The extrusion molding pressure when extruding the green clay is preferably 15 MPa or less, more preferably 10 MPa or less. It is preferred that the extrusion molding pressure is low, but from the viewpoint of ensuring strength, green clay that can be extruded at too low an extrusion molding pressure cannot be used. Therefore, the extrusion molding pressure is preferably 1 MPa or more, more preferably 3 MPa or more. Therefore, the extrusion molding pressure is, for example, preferably 1 to 15 MPa, more preferably 3 to 10 MPa.

[0082] Therefore, the green clay preferably contains an acrylic polymer and contains cross-linked starch under the condition that the P content is less than 0.2 parts by mass, preferably less than 0.1 parts by mass, and more preferably less than 0.05 parts by mass relative to 100 parts by mass of the ceramic raw material. The P content in the green clay can be less than 0.01 parts by mass, and further can be 0 parts by mass relative to 100 parts by mass of the ceramic raw material. From the viewpoint of achieving a high porosity while obtaining the strength improvement effect of the honeycomb structure, the lower limit of the content of the cross-linked starch in the green clay satisfies the preferred conditions of the above-mentioned P content, preferably 1 part by mass or more, more preferably 5 parts by mass or more, and further preferably 10 parts by mass or more relative to 100 parts by mass of the ceramic raw material. From the viewpoint of suppressing the generation of cracks caused by heat during firing, the upper limit of the content of the cross-linked starch in the green clay is preferably less than 50 parts by mass, more preferably less than 30 parts by mass, and further preferably less than 20 parts by mass relative to 100 parts by mass of the ceramic raw material.

[0083] When using starch cross-linked by a cross-linking agent containing P, even if the content of cross-linked starch in the clay is the same, the greater the degree of cross-linking, the greater the content of P, so the content of P can be used as an indicator of the degree of cross-linking. For example, as a cross-linked starch, a cross-linked starch having a P content of 0.01 mass part or more and less than 0.20 mass part per 10 mass parts of cross-linked starch can be used. The P content per 10 mass parts of cross-linked starch is preferably 0.01 mass part or more and less than 0.15 mass part, and more preferably 0.01 mass part or more and less than 0.1 mass part.

[0084] The P content in the green clay is determined by the following method. First, a sample (0.5 to 5.0 g) is collected from the green clay. Sulfuric acid is added to each sample and heated. After ashing, the sample solution is dissolved in hydrochloric acid. The sample solution is sprayed into a high-temperature argon plasma generated by high-frequency energy, and the emission intensity of the characteristic wavelength of the excited P atoms is measured by a sequential inductively coupled plasma emission spectrometer (ICP-OES / AES), which is converted into the P content in the green clay.

[0085] From the viewpoint of achieving high porosity while obtaining the effect of improving the strength of the honeycomb structure, the green clay preferably contains 0.5 parts by mass or more of an acrylic polymer, more preferably 0.7 parts by mass or more of an acrylic polymer, and further preferably 1.0 parts by mass or more of an acrylic polymer, relative to 100 parts by mass of the ceramic raw material. In addition, from the viewpoint of fluidity, the green clay preferably contains 10.0 parts by mass or less of an acrylic polymer, more preferably 7.0 parts by mass or less of an acrylic polymer, and further preferably 5.0 parts by mass or less of an acrylic polymer, relative to 100 parts by mass of the ceramic raw material. Therefore, the green clay, for example, preferably contains 0.5 parts by mass or more and 10 parts by mass or less of an acrylic polymer, more preferably 0.7 to 7.0 parts by mass of an acrylic polymer, and further preferably 1.0 to 5.0 parts by mass of an acrylic polymer, relative to 100 parts by mass of the ceramic raw material.

[0086] The type of acrylic polymer is not limited, and examples thereof include polyacrylic acid, polymethacrylic acid, polyacrylate, polymethacrylate, etc., and polymethyl methacrylate (PMMA) is particularly suitable as one type of acrylic polymer. The acrylic polymer may be cross-linked. One type of acrylic polymer may be used alone, or two or more types may be used in combination.

[0087] One or more other known pore-forming materials may be appropriately added to the clay, such as wheat flour, foamed resin, water-absorbent resin, uncrosslinked starch, porous silica, carbon (e.g., graphite), ceramic balls, polyethylene, polystyrene, polypropylene, nylon, polyester, phenol and other organic pore-forming materials.

[0088] From the perspective of affecting the strength of the honeycomb structure, pore-forming materials such as cross-linked starch and acrylic polymers are preferably used materials whose particle size has been adjusted by crushing, screening, etc. Specifically, in the volume-based cumulative particle size distribution measured by the laser diffraction scattering method, the lower limit of the cumulative 50% particle size (D50) of each pore-forming material from the small particle side is preferably 0.1 μm or more, more preferably 1.0 μm or more, and further preferably 5.0 μm or more. In addition, the upper limit of the cumulative 50% particle size (D50) of each pore-forming material from the small particle side is preferably 30.0 μm or less, more preferably 20.0 μm or less, and further preferably 15.0 μm or less. Therefore, for example, the cumulative 50% particle size (D50) of each pore-forming material from the small particle side is preferably 0.1 to 30.0 μm, more preferably 1.0 to 20.0 μm, and further preferably 5.0 to 15.0 μm.

[0089] As the binder, organic binders such as methylcellulose, hydroxypropyl methylcellulose, hydroxyethyl cellulose, carboxymethyl cellulose, polyvinyl alcohol, etc. can be exemplified. It is particularly preferred to use methylcellulose and hydroxypropyl methylcellulose in combination. In addition, from the viewpoint of improving the strength of the honeycomb formed body, the content of the binder in the green clay is preferably more than 4 parts by mass, more preferably more than 5 parts by mass, and more preferably more than 6 parts by mass relative to 100 parts by mass of the ceramic raw material. From the viewpoint of suppressing the cracking caused by abnormal heating in the firing process, the content of the binder in the green clay is preferably less than 9 parts by mass, more preferably less than 8 parts by mass, and more preferably less than 7 parts by mass relative to 100 parts by mass of the ceramic raw material. One type of binder can be used alone, or two or more types can be used in combination.

[0090] As the dispersion medium, water or a mixed solvent of water and an organic solvent such as alcohol can be cited, and water is particularly preferably used. The content of the dispersion medium in the green clay is preferably 30 to 70 parts by mass, more preferably 35 to 65 parts by mass, and further preferably 40 to 60 parts by mass relative to 100 parts by mass of the ceramic raw material. By making the content of the dispersion medium in the green clay 30 parts by mass or more relative to 100 parts by mass of the ceramic raw material, it is easy to obtain the advantage of easy stability of the quality of the honeycomb formed body. By making the content of the dispersion medium in the green clay 70 parts by mass or less relative to 100 parts by mass of the ceramic raw material, the shrinkage during drying becomes smaller and deformation can be suppressed. In this specification, the water content of the green clay refers to the value measured by the drying loss method.

[0091] The dispersant may be ethylene glycol, dextrin, fatty acid soap, polyether polyol, etc. The dispersant may be used alone or in combination of two or more. The content of the dispersant in the clay is preferably 0 to 2 parts by mass based on 100 parts by mass of the ceramic raw material.

[0092] (2-2. Drying of Honeycomb Formed Body)

[0093] Next, the honeycomb formed body is dried to obtain a honeycomb dried body. In the drying step, for example, a conventionally known drying method such as hot air drying, microwave drying, dielectric drying, reduced pressure drying, vacuum drying, freeze drying, etc. can be used. Among them, from the aspect of being able to quickly and evenly dry the entire formed body, a drying method combining hot air drying with microwave drying or dielectric drying is preferred. In addition, an intermittent dryer can be used, and a continuous dryer can also be used.

[0094] In the case of forming a sealing portion, after the sealing portion is formed at predetermined positions of the first bottom surface and the second bottom surface of the dried honeycomb formed body, the sealing portion is dried. The method for sealing the first bottom surface and the second bottom surface of the honeycomb formed body is not particularly limited, and a known method can be used. There is no particular restriction on the material of the sealing portion, and ceramics are preferably used from the viewpoint of strength and heat resistance. As a ceramic, it is preferably a ceramic material containing at least one selected from the group consisting of cordierite, mullite, zircon, aluminum titanate, silicon carbide, silicon nitride, zirconium oxide, spinel, India stone, sapphire, corundum and titanium dioxide. In order to make the expansion coefficients during firing the same and to improve durability, the material composition of the sealing portion is more preferably the same as that of the main body of the honeycomb formed body.

[0095] (2-3. Firing of Dried Honeycomb Body)

[0096] After the honeycomb molded body is dried, degreasing and sintering are performed to produce a columnar honeycomb structure. The conditions of the degreasing step and the sintering step can be known conditions according to the material composition of the honeycomb molded body and need not be specifically explained, but examples of specific conditions are given below.

[0097] The degreasing process is described. The combustion temperature of the binder is about 200°C, and the combustion temperature of the pore-forming material is about 300-1000°C. Therefore, the degreasing process can be carried out by heating the honeycomb molded body to a range of about 200-1000°C. The heating time is not particularly limited, but is usually about 10 hours to 100 hours. The honeycomb molded body after the degreasing process is called a calcined body.

[0098] The calcining step also depends on the material composition of the honeycomb formed body, and can be performed, for example, by heating the calcined body to 1350 to 1600° C. and maintaining the temperature for 3 to 10 hours.

[0099] When a honeycomb structure is used as a catalyst carrier, a catalyst can be supported on the partition walls. The method of supporting the catalyst on the porous partition walls is not particularly limited, and a known method can be adopted. For example, a method of contacting a catalyst composition slurry with the porous partition walls and then drying and firing can be cited. The catalyst composition slurry preferably contains one or a combination of two or more appropriate catalysts according to its use.

[0100] Examples

[0101] Hereinafter, examples for better understanding the present invention and its advantages are illustrated, but the present invention is not limited to the examples.

[0102] <A. Manufacture of honeycomb structures related to examples and comparative examples>

[0103] (1) Raw materials

[0104] As cordierite raw materials, talc, kaolin, alumina, aluminum hydroxide, and silica were prepared. Their volume-based cumulative 50% particle diameters (D50) measured by the laser diffraction scattering method are shown in Table 1.

[0105] As pore-forming materials, acrylic polymers, low-crosslinked starches, medium-crosslinked starches, and high-crosslinked starches were prepared. As the acrylic polymer, polyacrylic acid was used. The low-crosslinked starch, medium-crosslinked starch, and high-crosslinked starch are all starches crosslinked with a phosphoric acid-based crosslinking agent, but the degree of crosslinking is different. Their volume-based cumulative 50% particle diameters (D50) measured by the laser diffraction scattering method are shown in Table 1.

[0106] As additives, a binder, a dispersant, and water were prepared. Methyl cellulose was used as the binder, and ethylene glycol was used as the dispersant.

[0107] (2) Production of honeycomb green bodies

[0108] The raw material compositions prepared by mixing the above cordierite raw materials, pore-forming materials, and additives at the mass ratios shown in Table 1 according to the numbers of the examples and comparative examples were kneaded to form the green bodies of the examples and comparative examples, respectively. Table 1 shows the P content in the green bodies measured by the above method relative to 100 parts by mass of the ceramic raw materials.

[0109] Then, each green body was put into an extrusion molding machine and extruded through a die of a predetermined shape to obtain a cylindrical honeycomb green body. The pressure during extrusion molding (extrusion molding pressure) was measured using a pressure sensor. The results are shown in Table 1. After dielectric drying and hot air drying of the obtained honeycomb green body, the two bottom surfaces were cut to a predetermined size, and further hot air drying was performed under the conditions of 70°C × 2 hours.

[0110] (3) Firing

[0111] Next, heat degreasing was carried out at about 200°C in an air atmosphere, and then sintering was carried out at 1400°C for 10 hours in an air atmosphere to obtain the honeycomb structures of the examples and comparative examples. Manufacture the honeycomb structures in the quantities required for the following tests.

[0112] (4) Specifications of the honeycomb structure

[0113] The specifications of the obtained honeycomb structures are as follows.

[0114] Overall shape: cylindrical with a diameter of 100 mm × a height of 100 mm

[0115] Cell shape in the cross-section perpendicular to the flow path direction of the cells: square

[0116] Thickness of the partition wall (nominal value based on the die specifications): shown in Table 1

[0117] Cell density (number of cells per unit cross-sectional area): shown in Table 1 (cpsi: cells per square inch)

[0118] <B. Characteristic evaluation>

[0119] Various characteristic evaluations were performed on each of the honeycomb structures related to the above-obtained examples and comparative examples.

[0120] (1) Porosity

[0121] Partition wall samples (cubes with a length × width × height of approximately 13 mm × approximately 13 mm × approximately 13 mm) were collected from two locations near the radial center and near the outer periphery at the central part in the height direction of each honeycomb structure, and the porosity was measured by the mercury intrusion method, and the average value was taken as the measured value. The results are shown in Table 1.

[0122] (2) Measurement of isostatic crushing strength

[0123] Based on the automotive standard (JASO M505-87) issued by the Society of Automotive Engineers of Japan, the isostatic crushing strength of each honeycomb structure was measured. The results are shown in Table 1.

[0124] (3) Measurement of P content

[0125] The P content in each honeycomb structure was measured according to the above measurement method. The results are shown in Table 1.

[0126] [Table 1]

[0127]

[0128] (4) Discussion

[0129] The honeycomb structures involved in the embodiments and comparative examples are all thin-walled and have high porosity. Comparative Examples 1 to 6 are all examples in which only one of an acrylic acid polymer and a cross-linked starch is used as a pore-forming material. The strength of the honeycomb structures of Comparative Examples 1 to 4 is insufficient. Comparative Examples 5 and 6 using highly cross-linked starch have excellent strength, but the P content increases, and the extrusion molding pressure is too high, thereby significantly reducing the extrusion speed, and placing an excessive burden on the molding machine. On the other hand, in Examples 1 to 16, by using both an acrylic acid polymer and a cross-linked starch as pore-forming materials, a honeycomb structure with thin walls, high porosity and excellent strength can be manufactured without placing an excessive burden on the extrusion molding machine (the extrusion molding pressure is below 15 MPa).

Claims

1. A method for manufacturing a honeycomb structure, the honeycomb structure comprising an outer peripheral side wall and partition walls, the partition walls being arranged on the inner peripheral side of the outer peripheral side wall and dividing a plurality of cells forming a flow path from a first bottom surface to a second bottom surface, The method for manufacturing the honeycomb structure comprises: A step of extruding a clay material containing a ceramic raw material, a pore-forming material, a binder, and a dispersion medium through a die defining the opening shape of the plurality of cells, thereby producing a honeycomb molded body. a step of drying the honeycomb formed body to obtain a honeycomb dried body, and The step of firing the dried honeycomb body to obtain a honeycomb fired body having a partition wall thickness of 50 μm or more and 210 μm or less and a partition wall porosity of 45% to 60%; The pore-forming material in the clay contains cross-linked starch and acrylic acid polymer. The kneaded clay contains 1.0 part by mass or more of cross-linked starch based on 100 parts by mass of the ceramic raw material, under the condition that the P content is less than 0.2 parts by mass.

2. The manufacturing method according to claim 1, wherein: The kneaded clay contains 1.0 part by mass or more of cross-linked starch based on 100 parts by mass of the ceramic raw material, under the condition that the P content is 0.1 part by mass or less.

3. The manufacturing method according to claim 1, wherein: The kneaded clay contains 1.0 part by mass or more of cross-linked starch based on 100 parts by mass of the ceramic raw material under the condition that the P content is 0.05 parts by mass or less.

4. The production method according to any one of claims 1 to 3, wherein The P content in the honeycomb structure is less than 0.2 mass %.

5. The production method according to any one of claims 1 to 3, wherein The P content in the honeycomb structure is 0.1 mass % or less.

6. The production method according to any one of claims 1 to 3, wherein The P content in the honeycomb structure is 0.05 mass % or less.

7. The production method according to any one of claims 1 to 3, wherein The kneaded clay contains 0.5 parts by mass or more of an acrylic polymer based on 100 parts by mass of the ceramic raw material.

8. The production method according to any one of claims 1 to 3, wherein The ceramic raw material is a cordierite raw material.

9. A honeycomb structure having a peripheral side wall and partition walls, The partition wall is disposed on the inner peripheral side of the outer peripheral side wall and divides a plurality of cells that form a flow path from the first bottom surface to the second bottom surface. The thickness of the partition wall is 50 μm or more and 210 μm or less, The porosity of the partition wall is 45% to 60%. The P content in the honeycomb structure is 0.01 mass % or more and less than 0.2 mass %, and the isostatic fracture strength is 1.0 MPa or more.

10. The honeycomb structure according to claim 9, wherein: The upper limit of the P content in the honeycomb structure is 0.1 mass % or less.

11. The honeycomb structure according to claim 9, wherein The upper limit of the P content in the honeycomb structure is 0.05 mass % or less.

12. The honeycomb structure according to any one of claims 9 to 11, wherein The outer peripheral side walls and partition walls contain cordierite.

Citation Information

Patent Citations

  • Method for preparing crosslinked starch by utilizing sodium trimetaphosphate crosslinking agent

    CN105418774A

  • Ceramic porous body and method for producing the same, and dust collecting filter

    CN111747751A

  • Cordierite-containing ceramic bodies, batch composition mixtures, and methods of manufacturing cordierite-containing ceramic bodies

    CN113272042A

  • Method for producing porous ceramic article

    US20040051196A1

  • Honeycomb structure and method for manufacturing the same

    US20090274867A1