Preparation method of silver-titanium dioxide nano composite material and application of silver-titanium dioxide nano composite material in leather cultural relic protection
By preparing silver-titanium dioxide nanocomposites and utilizing their ultraviolet shielding, antibacterial and antioxidant properties, the problem of traditional leather cultural relic protection technology being complex and harmful to cultural relics has been solved, and a green and effective protection effect has been achieved.
Patent Information
- Application Number
- CN202410932761.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-12
AI Technical Summary
Traditional leather cultural relic protection technology has problems such as complicated preparation, unsatisfactory results and secondary damage to cultural relics. In particular, traditional detergents and reinforcement materials may cause color changes on the surface of cultural relics, material embrittlement and chemical corrosion.
Using the preparation method of silver-titanium dioxide nanocomposites, by mixing silver nitrate and chestnut tannin solution, and adding n-butyl titanate in a hydrothermal reaction, a silver-titanium dioxide nanocomposite is formed, taking advantage of its excellent ultraviolet shielding, Antibacterial and antioxidant properties protect leather artifacts.
This method reduces the generation of harmful substances in chemical synthesis, simplifies the preparation process, provides a green protection solution, has excellent ultraviolet shielding capabilities, prevents leather deterioration and fading, and maintains the original texture and appearance of cultural relics, with stable physical and Chemical properties, suitable for a wide range of leather cultural relic protection needs.
Smart Images

Figure BDA0004940257970000071 
Figure HDA0004940257980000011 
Figure HDA0004940257980000012
Abstract
Description
Technical Field
[0001] The invention belongs to the application field of cultural relics protection, and specifically discloses a preparation method of a silver-titanium dioxide nanocomposite material and application of the silver-titanium dioxide nanocomposite material in leather cultural relics protection. Background Art
[0002] As an important part of cultural heritage, leather cultural relics carry rich historical, cultural and artistic values. However, during the long-term preservation process, leather materials are easily corroded by factors such as light, oxidation, and microorganisms, resulting in discoloration, corruption and aging. Traditional cultural relic protection technologies usually rely on chemical protective agents, such as detergents, reinforcing agents, and mounting adhesives. Among them, detergents include water, organic solvents, oxidants (such as chloramine T, hydrogen peroxide, hypochlorite, chlorine dioxide), etc.; reinforcing agents generally use cellulose ethers, acrylic resins, fluororesins, Palaren and other reinforcing agents or plastic films and screens and other reinforcing materials; mounting adhesives include starch paste, carboxymethyl cellulose, cellulose diacetate, etc., which are used to repair organic cultural relics such as paper and silk. In addition, polymer materials can also be used as reinforcing materials, bonding materials, surface sealing materials, etc. in cultural relic protection, including natural organic polymer materials (such as polysaccharides, proteins, waxes, etc.) and synthetic resins (such as water-soluble synthetic resins, solvent-based synthetic resins, reactive polymer materials, polymer resin emulsions, etc.).
[0003] However, these methods often have certain limitations, such as complex preparation, unsatisfactory results, and secondary damage to cultural relics. Specifically, traditional detergents, due to their strong oxidizing properties, can cause color changes on the surface of cultural relics, embrittlement of the material, and potential chemical corrosion; reinforcement materials such as acrylic resins have poor weather resistance, are prone to failure, and may degrade into harmful small molecules. Therefore, for biomass-based cultural relics, especially leather cultural relics, traditional protective materials and methods may change the texture and appearance of the cultural relics, affecting their historical value. Summary of the invention
[0004] In view of the problems and shortcomings of the prior art, the present invention provides a silver-titanium dioxide nanocomposite material suitable for the protection of leather cultural relics, and also provides a corresponding preparation method.
[0005] Based on the above purpose, the present invention adopts the following technical solution:
[0006] In a first aspect, the present invention provides a method for preparing a silver-titanium dioxide nanocomposite material, comprising the following steps:
[0007] (1) mixing a silver nitrate solution with a chestnut tannin solution to obtain a silver nitrate-chestnut tannin solution;
[0008] (2) dissolving n-butyl titanate in anhydrous ethanol to obtain an n-butyl titanate solution, adding the n-butyl titanate solution to the silver nitrate-chestnut extract solution and mixing them evenly to obtain a mixed solution;
[0009] (3) subjecting the mixed solution to a hydrothermal reaction, and after the reaction is completed, centrifuging, washing, drying, and calcining to obtain a silver-titanium dioxide nanocomposite material.
[0010] Preferably, the mass fraction of silver nitrate in the silver nitrate solution of step (1) is 1% to 10%, and the mass fraction of chestnut tannin in the chestnut tannin solution is 5% to 15%; the weight ratio of the silver nitrate solution to the chestnut tannin solution is (0.5 to 5.0):1.0.
[0011] Preferably, the weight ratio of n-butyl titanate to anhydrous ethanol in step (2) is 1:(10-30).
[0012] More preferably, the weight ratio of the n-butyl titanate solution to the silver nitrate-chestnut tannin solution is (10-30):1.
[0013] More preferably, the mixing time is 30 minutes.
[0014] Preferably, the hydrothermal reaction temperature in step (3) is 120-160° C. and the reaction time is 2-6 hours.
[0015] More preferably, the hydrothermal reaction vessel is a stainless steel reactor lined with polytetrafluoroethylene.
[0016] More preferably, the centrifugal speed is 3000-6000 rpm, and the time is 20-60 min.
[0017] More preferably, the cleaning process is: cleaning with deionized water and ethanol three times respectively.
[0018] More preferably, the drying temperature is 100-150° C. and the drying time is 10-20 hours.
[0019] More preferably, the calcination temperature is 300-800° C. and the calcination time is 1-5 hours.
[0020] In a second aspect, the present invention provides a silver-titanium dioxide nanocomposite material prepared by the preparation method described in the first aspect.
[0021] In a third aspect, the present invention provides application of the silver-titanium dioxide nanocomposite material described in the second aspect in the protection of leather cultural relics.
[0022] In a fourth aspect, the present invention provides a method for applying the silver-titanium dioxide nanocomposite material described in the second aspect in the protection of leather cultural relics, which is: ultrasonically dispersing the silver-titanium dioxide nanocomposite material in water to obtain a dispersed solution, and spraying or immersing the dispersed solution on the surface of the leather cultural relic.
[0023] Preferably, the weight ratio of the silver-titanium dioxide nanocomposite material to water is 1:1000-4000.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The present invention uses chestnut tannin extract in chestnut extract as a template. Chestnut tannin extract not only has a specific polyphenol structure, but also can be used as a template to promote the formation of titanium dioxide nanoparticles and can also be used as a reducing agent to convert Ag + The silver particles are reduced to nano silver particles, and the silver particles serve as the nuclei for the growth of titanium dioxide to prepare silver-titanium dioxide nanoparticles. At the same time, the addition of chestnut wood and silver can reduce the particle size of the nanoparticles, help control the shape and size of the particles, increase the specific surface area, and thus improve its photocatalytic activity and ability to absorb ultraviolet light.
[0026] 2. The chestnut tannin extract used in the present invention is a natural biological resource. The preparation process reduces the harmful substances that may be produced in the chemical synthesis method, belongs to green synthesis preparation, and reduces the risk of environmental pollution. At the same time, the chestnut tannin extract is used as a template to make TiO 2 Synthesis and Ag + The reduction is completed in the same step, which simplifies the preparation process of titanium dioxide nanoparticles. Compared with the sol-gel method, the preparation time cost can be greatly shortened.
[0027] 3. The silver-titanium dioxide nanocomposite material of the present invention has excellent ultraviolet shielding ability, which prevents the deterioration and fading of leather caused by ultraviolet radiation; the present invention has excellent antibacterial properties, which can effectively prevent the corruption, mildew and other problems of leather cultural relics caused by microbial invasion; the present invention has good antioxidant properties, which can effectively prevent the leather cultural relics from losing their original color and texture due to oxidation reactions; the present invention has stable physical and chemical properties, and can maintain its performance under various environmental conditions; the present invention takes into account the problem of minimizing the impact on the texture and appearance of leather cultural relics, and the fine structure and distribution of the silver-titanium dioxide nanocomposite material ensure that the original texture of the leather cultural relics will not be destroyed.
[0028] 4. The present invention provides a flexible preparation scheme based on formula design, which allows the ratio of silver and titanium dioxide to be adjusted during the preparation process to meet the needs of different cultural relics protection. This feature enables the present invention to be applied in a wide range of leather cultural relics protection and restoration projects, with high flexibility and applicability. This wide applicability makes the present invention have greater application potential in the field of cultural relics protection and can meet the protection needs of different types of leather cultural relics. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 (A, a) is a transmission electron microscopy image of the titanium dioxide nanomaterial prepared in Comparative Example 1, Figure 1 (B, b) is a transmission electron microscopy image of the titanium dioxide nanomaterial prepared in Comparative Example 2. Figure 1 (C, c) are transmission electron microscopy images of the silver-titanium dioxide nanocomposite prepared in Example 1;
[0030] Figure 2 (A, a) is a scanning electron microscope image of the titanium dioxide nanomaterial prepared in Comparative Example 1, Figure 2 (B, b) is a scanning electron microscope image of the titanium dioxide nanomaterial prepared in Comparative Example 2, Figure 2 (C, c) is a scanning electron microscope image of the silver-titanium dioxide nanocomposite prepared in Example 1, Figure 2 (c1, c2, c3) are element distribution diagrams of Ti, O, and Ag on the surface of the silver-titanium dioxide nanocomposite material prepared in Example 1;
[0031] Figure 3 X-ray diffraction (XRD) spectra of the nanomaterials prepared in Example 1 and Comparative Examples 1-2;
[0032] Figure 4 The particle size distribution diagram of the silver-titanium dioxide nanocomposite material prepared in Example 1 and Comparative Example 3;
[0033] Figure 5 (A, a) is a transmission electron microscopy image of the titanium dioxide nanomaterial prepared in Comparative Example 1, Figure 5 (B, b) is a transmission electron microscopy image of the silver-titanium dioxide nanocomposite material prepared in Example 1, Figure 5 (C, c) is a transmission electron microscopy image of the silver-titanium dioxide nanocomposite prepared in Example 2, Figure 5 (D, d) is a transmission electron microscopy image of the silver-titanium dioxide nanocomposite prepared in Comparative Example 4;
[0034] Figure 6 The ultraviolet shielding performance test results of the nanomaterials prepared in Examples 1, 3, 4, and Comparative Examples 1 and 2 are shown;
[0035] Figure 7The antioxidant capacity test results of the nanomaterials prepared in Examples 1, 3, 4, and Comparative Examples 1 and 2 are shown;
[0036] Figure 8 The particle size distribution diagram of the nanomaterials prepared in Examples 1, 3, 4, and Comparative Examples 1 and 2;
[0037] Fig. 9 The antibacterial performance test results of the nanomaterials prepared in Examples 1, 3, 4 and Comparative Example 2 are shown;
[0038] Fig.10 This is a comparison chart of the surface color difference and antibacterial ability of the leather before and after treatment in Example 5. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solution and advantages of the present invention clearer and more specific, the present invention is further described in detail by examples below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0040] Example 1
[0041] A silver-titanium dioxide nanocomposite material, the preparation method thereof has the following steps:
[0042] (1) dissolving silver nitrate in deionized water to obtain a silver nitrate solution with a mass fraction of 2%, dissolving chestnut tannin extract in deionized water, centrifuging and filtering to obtain a chestnut tannin extract solution with a mass fraction of 10%; mixing the silver nitrate solution and the chestnut tannin extract solution in a volume ratio of 1:2 to obtain a silver nitrate-chestnut tannin extract solution;
[0043] (2) dissolving 1 mL of n-butyl titanate in anhydrous ethanol and adjusting the volume to 20 mL to obtain a n-butyl titanate solution; adding the obtained n-butyl titanate solution dropwise to 1.5 mL of silver nitrate-chestnut tannin solution, mixing at room temperature for 30 min, and obtaining a mixed solution;
[0044] (3) The mixed solution was transferred to a stainless steel reactor lined with polytetrafluoroethylene and subjected to a hydrothermal reaction at 140°C for 4 h. After the reaction was completed, the mixture was centrifuged at 4000 rpm for 30 min. The precipitate was washed with deionized water and ethanol three times, dried at 120°C for 16 h, and then calcined in a muffle furnace at 500°C for 3 h to obtain a silver-titanium dioxide nanocomposite material.
[0045] Comparative Example 1
[0046] A titanium dioxide nanomaterial, the preparation method thereof has the following steps:
[0047] (1) dissolving 1 mL of n-butyl titanate in anhydrous ethanol and adjusting the volume to 20 mL to obtain a n-butyl titanate solution; dropping 1 part of the n-butyl titanate solution into 50 parts of deionized water and mixing at room temperature for 30 minutes to obtain a mixed solution;
[0048] (2) The mixed solution was transferred to a stainless steel reactor lined with polytetrafluoroethylene and subjected to hydrothermal reaction at 140°C for 4 h. After the reaction, the mixture was centrifuged at 4000 rpm for 30 min. The precipitate was washed with deionized water and ethanol three times respectively, dried at 120°C for 16 h, and then calcined in a muffle furnace at 500°C for 3 h to obtain titanium dioxide nanomaterials.
[0049] Comparative Example 2
[0050] A titanium dioxide nanomaterial, the preparation method thereof has the following steps:
[0051] (1) dissolving chestnut tannin extract in deionized water, centrifuging and filtering to obtain a chestnut tannin extract solution with a mass fraction of 10%;
[0052] (2) dissolving 1 part of n-butyl titanate in 20 parts of anhydrous ethanol to obtain a n-butyl titanate solution; dropping all of the obtained n-butyl titanate solution into 1.5 mL of the chestnut tannin solution, mixing at room temperature for 30 minutes, and obtaining a mixed solution;
[0053] (3) The mixed solution was transferred to a stainless steel reactor lined with polytetrafluoroethylene and subjected to hydrothermal reaction at 140°C for 4 h. After the reaction, the mixture was centrifuged at 4000 rpm for 30 min. The precipitate was washed with deionized water and ethanol three times respectively, dried at 120°C for 16 h, and then calcined in a muffle furnace at 500°C for 3 h to obtain titanium dioxide nanomaterials.
[0054] The nanomaterials prepared in Example 1 and Comparative Examples 1-2 were subjected to transmission electron microscopy. The transmission electron microscopy results (TEM) are as follows: Figure 1 .in, Figure 1 (A, a) is a transmission electron microscopy image of the titanium dioxide nanomaterial prepared in Comparative Example 1, Figure 1 (B, b) is a transmission electron microscopy image of the titanium dioxide nanomaterial prepared in Comparative Example 2. Figure 1 (C, c) is a transmission electron microscopy image of the silver-titanium dioxide nanocomposite material prepared in Example 1.
[0055] from Figure 1 (A, B, C) It can be seen that nanomaterials are composed of small particles of tens of nanometers. Figure 1 (a, b) are HRTEM images of titanium dioxide nanoparticles with a lattice spacing of 0.35 nm, which is consistent with the (101) crystal plane of anatase titanium dioxide. Figure 1(c) is the HRTEM image of Ag, the interplanar spacing is 0.20 nm, which is consistent with the (200) interplanar spacing of silver.
[0056] The nanomaterials prepared in Example 1 and Comparative Examples 1-2 were subjected to scanning electron microscopy. Figure 2 .in, Figure 2 (A, a) is a scanning electron microscope image of the titanium dioxide nanomaterial prepared in Comparative Example 1, Figure 2 (B, b) is a scanning electron microscope image of the titanium dioxide nanomaterial prepared in Comparative Example 2, Figure 2 (C, c) is a scanning electron microscope image of the silver-titanium dioxide nanocomposite prepared in Example 1, Figure 2 (c1, c2, c3) are element distribution diagrams of Ti, O, and Ag on the surface of the silver-titanium dioxide nanocomposite material prepared in Example 1.
[0057] from Figure 2 (A, a) It can be seen that the size of the nanoparticles synthesized in Comparative Example 1 is about 200 nm, but they are prone to agglomeration. Figure 2 (B, b) It can be seen that the addition of chestnut wood extract in Comparative Example 2 can make the nanoparticles form shorter rod-shaped aggregates with more regular structure and more uniform particle size. Figure 2 (C, c) It can be seen that the addition of silver in Example 1 increases the surface roughness, provides more reaction sites, and helps to improve its reaction activity. Figure 2 The EDS spectra of (c1, c2, c3) show that the Ti, O, and Ag elements exist and are evenly dispersed in Example 1.
[0058] The nanomaterials prepared in Example 1 and Comparative Examples 1-2 were analyzed by XRD, and the crystallization of the nanoparticles was determined by their diffraction peaks. The results are as follows: Figure 3 As shown. Among them, TiO 2 is the titanium dioxide nanomaterial prepared in Comparative Example 1, CT is the titanium dioxide nanomaterial prepared in Comparative Example 2, and CTA is the silver-titanium dioxide nanocomposite material prepared in Example 1.
[0059] from Figure 3It can be seen that the peaks of titanium dioxide prepared in Example 1 and Comparative Examples 1-2 are 25.3°, 37.8°, 48.0°, 53.9°, 55.1°, 62.7°, 68.8°, 70.3° and 75.1°, which correspond to the crystal planes (101), (004), (200), (105), (211), (204), (116) and (220) of anatase titanium dioxide, respectively. In addition, the silver-titanium dioxide nanocomposite material synthesized in Example 1 has diffraction peaks of 38.1°, 44.3°, 64.5° and 77.4°, which correspond to the crystal planes (111), (200), (220) and (311) of silver, respectively.
[0060] Figure 1 , 2 3 can be explained that the nanomaterials prepared in Example 1 and Comparative Examples 1-2 are titanium dioxide with anatase structure. The crystal structure of the composite material is an important factor determining its photoreaction efficiency. Among the two most common crystal forms of titanium dioxide, the photoreaction activity of anatase crystal is relatively high compared with rutile crystal. In addition, Example 1 has silver nanoparticles with a face-centered cubic (fcc) structure, indicating successful silver doping.
[0061] Comparative Example 3
[0062] A silver-titanium dioxide nanocomposite material, the preparation method thereof has the following steps:
[0063] (1) dissolving silver nitrate in deionized water to obtain a silver nitrate solution with a mass fraction of 2%, dissolving quebracho extract in deionized water, centrifuging and filtering to obtain a quebracho extract solution with a mass fraction of 10%; mixing the silver nitrate solution and the quebracho extract solution in a volume ratio of 1:2 to obtain a silver nitrate-quebracho extract solution;
[0064] (2) dissolving 1 ml of n-butyl titanate in anhydrous ethanol and adjusting the volume to 20 ml to obtain a n-butyl titanate solution; dropping the obtained n-butyl titanate solution into 1.5 ml of silver nitrate-quebracho tannin solution, mixing at room temperature for 30 min, and obtaining a mixed solution;
[0065] (3) The mixed solution was transferred to a stainless steel reactor lined with polytetrafluoroethylene and subjected to a hydrothermal reaction at 140°C for 4 h. After the reaction was completed, the mixture was centrifuged at 4000 rpm for 30 min. The precipitate was washed with deionized water and ethanol three times, dried at 120°C for 16 h, and then calcined in a muffle furnace at 500°C for 3 h to obtain a silver-titanium dioxide nanocomposite material.
[0066] The particle sizes of the silver-titanium dioxide nanocomposites prepared in Example 1 and Comparative Example 3 were measured using a dynamic light scattering method. The results are as follows: Figure 4 .
[0067] from Figure 4 It can be seen that compared with Comparative Example 1, the titanium dioxide molecular particle size synthesized by chestnut wood extract is smaller and the particle size distribution is narrower. This is because the quebracho extract (quebracho tannin extract) is a condensation tanning agent, which is prone to condensation and hydrolysis reactions when heated. On the one hand, it will form a larger molecular particle size, resulting in a larger particle size of the titanium dioxide molecular particle size using it as a template, and on the other hand, it will decompose into small molecular phenolic substances, ultimately resulting in a wider molecular weight distribution. Chestnut wood extract (chestnut tannin extract) is a hydrolysis tanning agent, which will undergo a hydrolysis reaction when heated, thereby obtaining titanium dioxide with a smaller molecular particle size and a narrower particle size distribution, which helps to improve its photocatalytic activity and ability to absorb ultraviolet light.
[0068] Example 2
[0069] A silver-titanium dioxide nanocomposite material, whose components and preparation method are basically the same as those of Example 1, except that the mass fraction of chestnut tannin extract in the chestnut tannin extract solution in step (1) is 5%.
[0070] Comparative Example 4
[0071] A silver-titanium dioxide nanocomposite material, whose components and preparation method are basically the same as those of Example 1, except that the mass fraction of chestnut tannin extract in the chestnut tannin extract solution in step (1) is 20%.
[0072] (I) Electron microscope transmission test
[0073] The silver-titanium dioxide nanocomposites prepared in Examples 1, 2, and Comparative Examples 1 and 4 were subjected to electron microscopy transmission. The transmission results are shown in FIG. Figure 5 .in, Figure 5 (A, a) is a transmission electron microscopy image of the titanium dioxide nanomaterial prepared in Comparative Example 1, Figure 5 (B, b) is a transmission electron microscopy image of the silver-titanium dioxide nanocomposite material prepared in Example 1, Figure 5 (C, c) is a transmission electron microscopy image of the silver-titanium dioxide nanocomposite prepared in Example 2, Figure 5 (D, d) is a transmission electron microscopy image of the silver-titanium dioxide nanocomposite material prepared in Comparative Example 4.
[0074] from Figure 5 It can be seen that because the chestnut extract (chestnut tannin) contains rich hydroxyl groups that can change the surface properties of the particles, it affects the dispersibility of the nanoparticles. When the mass fraction of chestnut tannin is increased from 5% to 10%, it can be seen that the particles have good dispersibility and are easy to form micron-sized particles, but when the addition amount is increased to 20%, the nanoparticles are severely agglomerated and become a whole. Therefore, in the embodiment, when the mass fraction of chestnut tannin is 10%, the dispersibility of the particles is the best.
[0075] Example 3
[0076] A silver-titanium dioxide nanocomposite material, whose components and preparation method are basically the same as those of Example 1, except that the mass fraction of silver nitrate in the silver nitrate solution in step (1) is 6%.
[0077] Example 4
[0078] A silver-titanium dioxide nanocomposite material, whose components and preparation method are basically the same as those of Example 1, except that the mass fraction of silver nitrate in the silver nitrate solution in step (1) is 10%.
[0079] (II) UV shielding performance test
[0080] The nanomaterials prepared in Examples 1, 3, 4, and Comparative Examples 1 and 2 were tested for ultraviolet shielding performance using the ultraviolet-visible light diffuse reflection method. The test results are as follows: Figure 6 .
[0081] from Figure 6 It can be seen that the addition of chestnut tannin extract in Comparative Example 2 enhances the absorption capacity of the material in the visible light region compared with Comparative Example 1. In addition, in Examples 1, 3, and 4, as the silver content increases, the absorption capacity in the visible light range increases, while the absorption capacity in the ultraviolet range decreases.
[0082] The Kubelka-Munk equation was used to calculate the bandgap width of the synthesized nanoparticles. The formula is as follows:
[0083]
[0084] Among them, hv is the photon energy, α is the absorption coefficient, A is the proportional constant, and Eg is the band gap width. In a geometric sense, it represents the intercept of the linear part of the curve on the x-axis. For indirect band gap semiconductors, n=2.
[0085] Through calculation, it can be known that compared with comparative example 1, the addition of chestnut extract in comparative example 2 reduces Eg from 3.2eV to 3.18eV. In Examples 1, 3, and 4, as the Ag content increases, the band gap becomes smaller, which is beneficial to the utilization of visible light by nanoparticles. When the mass fraction of silver nitrate is 10%, Eg drops to 2.79eV, which means that it can absorb light with a wavelength of less than 444nm, and its ability to utilize visible light is greatly increased. In addition, due to the conductivity of Ag, the recombination of electron holes is reduced, the bandgap width of the material is reduced, and the light response area is widened, which is more conducive to the utilization of sunlight and the generation of photogenerated carriers, thereby improving the photocatalytic activity.
[0086] (III) Antioxidant capacity test
[0087] The nanomaterials prepared in Examples 1, 3, 4, and Comparative Examples 1 and 2 were subjected to a DPPH free radical scavenging method to measure their DPPH free radical scavenging ability, i.e., antioxidant ability. The measurement results are as follows: Figure 7 .
[0088] from Figure 7 It can be seen that the addition of chestnut tannin extract in Comparative Example 2 enhances the antioxidant capacity of the material compared with Comparative Example 1. In addition, in Examples 1, 3, and 4, as the silver content increases, the antioxidant capacity increases. When the mass fraction of silver nitrate reaches 6%, a higher antioxidant capacity can be obtained, while when the mass fraction of silver nitrate reaches 10%, the antioxidant capacity does not increase significantly.
[0089] (IV) Antibacterial performance test
[0090] The particle sizes of the nanomaterials prepared in Examples 1, 3, 4 and Comparative Examples 1 and 2 were measured by dynamic light scattering. The results are as follows: Figure 8 .
[0091] from Figure 8 It can be seen that titanium dioxide nanoparticles can aggregate into aggregates of about 200 nm. Compared with comparative example 1, the size distribution of nanoparticles in comparative example 2 becomes wider with the addition of chestnut wood extract template. This is because under heating conditions, chestnut wood extract undergoes hydrolysis reaction, which broadens the molecular weight distribution. In Examples 1, 3, and 4, the addition of silver effectively improves this situation because Ag + It is easier to reduce to nano-Ag particles and become the nucleus for the growth of titanium dioxide crystals. + With the increase of content, the number of crystal nuclei increases, and the amount of n-butyl titanate participating in the reaction on each crystal nucleus decreases, which reduces the grain size.
[0092] The nanomaterials prepared in Examples 1, 3, 4 and Comparative Example 2 were tested for their antibacterial properties using the inhibition zone observation method. The test results are as follows: Fig. 9 .
[0093] from Fig. 9 It can be seen that the silver-titanium dioxide nanocomposites prepared in Examples 1, 3 and 4 have antibacterial activity against two typical bacteria, Staphylococcus aureus and Escherichia coli. When the mass fraction of silver nitrate is 10%, the sizes of the inhibition zones against the two bacteria are 8.2 mm and 6.4 mm respectively.
[0094] Combination Figure 8 , 9Analysis shows that the key mechanism for silver-titanium dioxide nanocomposites to exert their antibacterial activity is through the release of silver ions, which can directly contact and kill bacterial cells, or indirectly participate by interacting with protein thiol groups, thereby destroying DNA and killing bacterial cells. The release rate of silver is proportional to the surface area of the particles. As the size of the nanoparticles decreases, the surface area increases, so smaller nanoparticles have a faster release rate, which improves their antibacterial properties. The antibacterial ability of nanoparticles can be controlled by adjusting the size and morphology of the nanoparticles.
[0095] Based on the above comprehensive evaluation, Example 4 is the optimal example.
[0096] Example 5
[0097] The application of silver-titanium dioxide nanocomposite materials in the protection of leather cultural relics is as follows:
[0098] The silver-titanium dioxide nanocomposite prepared in Example 1 was ultrasonically dispersed in water, wherein the weight ratio of the silver-titanium dioxide nanocomposite to water was 1:2500, to obtain a dispersed solution, which was then sprayed on the surface of the leather cultural relic.
[0099] (V) Comparison of leather before and after treatment
[0100] The surface color difference and antibacterial ability of leather before and after treatment were compared. The comparison results are as follows: Fig.10 .
[0101] Depend on Fig.10 It can be seen that after the dispersion was sprayed on the surface of the leather artifact, the color difference value of the leather artifact surface did not change significantly. Through the antibacterial performance test, it can be seen that the leather sprayed with the dispersion showed a more obvious antibacterial zone, indicating that the color difference of the leather surface treated with the silver-titanium dioxide nanocomposite material did not change significantly and had a significant antibacterial effect.
[0102] The above is a description of a preferred embodiment of the present invention, but it should be understood that the invention is not limited to the contents disclosed herein. As long as non-substantial improvements are made using the method concept and technical solution of the present invention, or the method concept and technical solution of the present invention are applied to other occasions, they are all within the scope of protection of the present invention.
Claims
1. A method for preparing a silver-titanium dioxide nanocomposite material, characterized in that: The steps include: (1) mixing a silver nitrate solution with a chestnut tannin solution to obtain a silver nitrate-chestnut tannin solution; (2) dissolving n-butyl titanate in anhydrous ethanol to obtain an n-butyl titanate solution, adding the n-butyl titanate solution to the silver nitrate-chestnut extract solution and mixing them evenly to obtain a mixed solution; (3) subjecting the mixed solution to a hydrothermal reaction, and after the reaction is completed, centrifuging, washing, drying, and calcining to obtain a silver-titanium dioxide nanocomposite material.
2. The method for preparing the silver-titanium dioxide nanocomposite material according to claim 1, characterized in that: The mass fraction of silver nitrate in the silver nitrate solution of step (1) is 1% to 10%, and the mass fraction of chestnut tannin in the chestnut tannin solution is 5% to 15%; the weight ratio of the silver nitrate solution to the chestnut tannin solution is (0.5 to 5.0):1.
0.
3. The method for preparing the silver-titanium dioxide nanocomposite material according to claim 1, characterized in that: In step (2), the weight ratio of n-butyl titanate to anhydrous ethanol is 1:(10-30).
4. The method for preparing the silver-titanium dioxide nanocomposite material according to claim 3, characterized in that: The weight ratio of the n-butyl titanate solution to the silver nitrate-chestnut tannin solution is (10-30):
1.
5. The method for preparing the silver-titanium dioxide nanocomposite material according to claim 1, characterized in that: The hydrothermal reaction temperature in step (3) is 120-160° C. and the reaction time is 2-6 hours.
6. The method for preparing the silver-titanium dioxide nanocomposite material according to claim 5, characterized in that: The calcination temperature is 300-800° C. and the calcination time is 1-5 hours.
7. The silver-titanium dioxide nanocomposite material prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the silver-titanium dioxide nanocomposite material as claimed in claim 7 in the protection of leather cultural relics.
9. The use of the silver-titanium dioxide nanocomposite material in the protection of leather cultural relics as claimed in claim 8, characterized in that: The application method comprises the following steps: ultrasonically dispersing the silver-titanium dioxide nanocomposite material in water to obtain a dispersed solution, and spraying or dipping the dispersed solution on the surface of the leather cultural relic.
10. The use of the silver-titanium dioxide nanocomposite material in the protection of leather cultural relics as claimed in claim 9, characterized in that: The weight ratio of the silver-titanium dioxide nanocomposite material to water is 1:(1000-4000).
Citation Information
Patent Citations
Functional adsorbent and its production method
JP2003199810A
Photocatalyst particle and method for producing same, material including said particle, and product including said material
WO2019160110A1
Multifunctional particle comprising titanium dioxide, silver, silicon dioxide
WO2024134540A1