High-temperature-resistant polyimide water-based carbon fiber sizing agent and preparation method thereof
The high-temperature-resistant polyimide water-based carbon fiber sizing agent prepared through aqueous phase polycondensation reaction and calcium ion coordination solves the problems of insufficient temperature resistance and the use of organic solvents in existing sizing agents, and achieves efficient carbon fiber modification and composite materials. Performance improvements.
Patent Information
- Application Number
- CN202411005351.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-01
AI Technical Summary
The existing sizing agent has insufficient temperature resistance and uses a large amount of organic solvents, which affects the environment and health. At the same time, it has poor bonding effect with carbon fiber.
A high-temperature resistant polyimide water-based carbon fiber sizing agent prepared from triethylamine, aromatic dianhydride, aromatic diamine and deionized water is used to enhance the surface wettability and phase properties of the carbon fiber through aqueous phase polycondensation reaction and calcium ion coordination. Capacity.
The environmentally friendly water-based sizing agent with high temperature resistance level has been realized, which improves the interfacial compatibility and bonding strength of carbon fiber and resin matrix, and enhances the overall performance and stability of composite materials.
Smart Images

Figure CN118727449A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a sizing agent and a preparation method thereof. Background Art
[0002] Carbon fiber resin-based composite materials have the advantages of extremely high specific stiffness, near-zero thermal expansion coefficient and excellent dimensional stability. They are widely used in the manufacture of key components of spacecraft, such as satellite center bearing tubes, solar wing substrates and Hubble Telescope optical platforms and other primary / secondary bearing structures. However, due to the high degree of graphitization and high surface chemical inertness of carbon fiber, the wettability and compatibility of carbon fiber with the resin matrix are poor, which greatly limits the efficiency of the specific stiffness of carbon fiber in composite materials. Modifying the surface of carbon fiber can improve its bonding ability with the matrix material, improve the performance of the composite material, and meet a wider range of application needs. At present, the main methods for modifying the surface of carbon fiber include surface oxidation, polymer grafting, plasma modification, high-energy beam irradiation and other methods. However, these methods have the disadvantages of high cost, complex process and possible impact on the intrinsic properties of carbon fiber.
[0003] The sizing method has become the most commonly used carbon fiber surface treatment method because of its advantages of reinforcing and protecting the fibers, simple process, fast and efficient, and suitable for industrial applications. Before the carbon fiber leaves the factory, a layer of sizing agent is coated on its surface. After drying, a uniform resin layer will form on the fiber surface. This layer of resin can not only protect the fiber and prevent the carbon fiber from fuzzing and breaking during processing, but also improve the wettability between the fiber and the resin, and increase the compatibility and bonding between the two. The water-based sizing agent can form a wrap on the surface of the carbon fiber to reduce fuzz, protect the fiber, and adjust the compatibility with the matrix resin. This method is simple and environmentally friendly.
[0004] At present, most commercial sizing agents are mainly epoxy resin sizing agents, which are not heat-resistant enough. When epoxy resin sizing agents are used in polyetheretherketone carbon fiber reinforced composites (CF / PEEK) and polyimide carbon fiber reinforced composites (CF / PI), high temperatures will cause the epoxy resin to decompose, forming holes and defects. Under the action of external forces, these defects cause stress concentration, accelerate the interface failure of the composite material, and reduce the performance of the composite material.
[0005] Domestic and foreign researchers have actively explored the preparation of thermoplastic sizing agents suitable for PI matrices and have achieved some results. The PI thermoplastic sizing agents they developed can be matched with polyimide resin matrices. This is because the structure of these resins is similar to that of PI, so they have good compatibility and molecular entanglement with the PI matrix. In addition, some research works further enhance the interfacial interaction between CF and PI resin by establishing chemical bonds, hydrogen bonds and π-π interactions between the sizing layer on the CF surface and the PI matrix. However, most of the above-mentioned sizing agents use organic solvents as dispersion media. Organic solvents not only increase the manufacturing cost of the sizing agent, but also have adverse effects on the environment and the health of production operators. The developed PI thermoplastic sizing agent has poor bonding effect with carbon fiber. Therefore, it is of great significance to develop a green and environmentally friendly water-based sizing agent with high temperature resistance. Summary of the invention
[0006] The present invention aims to solve the problems that the existing sizing agent has insufficient temperature resistance, and the PI thermoplastic sizing agent uses a large amount of organic solvents and has poor bonding effect with carbon fibers, and further provides a high temperature resistant polyimide water-based carbon fiber sizing agent and a preparation method thereof.
[0007] A high temperature resistant polyimide water-based carbon fiber sizing agent is prepared from triethylamine, aromatic dianhydride, aromatic diamine, deionized water and calcium chloride; the molar ratio of the aromatic dianhydride to the aromatic diamine is 1:(0.9-2); the molar ratio of the aromatic dianhydride to the calcium chloride is 1:(1.9-2.2);
[0008] The aromatic diamine is 4,4'-bis(4-amino-2-trifluoromethylphenoxy)biphenyl or 4,4'-bis(3-aminophenoxy)biphenyl;
[0009] The aromatic dianhydride is 2,2'-difluoromethyl-4,4',5,5'-biphenyltetracarboxylic dianhydride or 3,3',4,4'-biphenyltetracarboxylic dianhydride.
[0010] A method for preparing a high temperature resistant polyimide water-based carbon fiber sizing agent is carried out according to the following steps:
[0011] 1. Weigh triethylamine, aromatic dianhydride, aromatic diamine, deionized water and calcium chloride; the molar ratio of the aromatic dianhydride to the aromatic diamine is 1:(0.9-2); the molar ratio of the aromatic dianhydride to the calcium chloride is 1:(1.9-2.2);
[0012] The aromatic diamine is 4,4'-bis(4-amino-2-trifluoromethylphenoxy)biphenyl or 4,4'-bis(3-aminophenoxy)biphenyl;
[0013] The aromatic dianhydride is 2,2'-difluoromethyl-4,4',5,5'-biphenyltetracarboxylic dianhydride or 3,3',4,4'-biphenyltetracarboxylic dianhydride;
[0014] 2. In a nitrogen atmosphere, at a temperature of 30°C to 35°C and under stirring, triethylamine and aromatic diamine are added to deionized water to react to obtain a reaction solution, the reaction solution is heated to 40°C to 50°C, aromatic dianhydride is added to the reaction solution three times by mass, and the reaction is carried out in a nitrogen atmosphere, at a temperature of 80°C to 85°C and under stirring, and finally calcium chloride is added, and the reaction is carried out in a nitrogen atmosphere, at a temperature of 60°C to 65°C and under stirring to obtain a high temperature resistant polyimide water-based carbon fiber sizing agent.
[0015] The beneficial effects of the present invention are:
[0016] The present invention utilizes simple water phase polycondensation reaction to prepare high temperature resistant grade water-based sizing agent, only requires simple stirring and heating device, and the method process is easy to control and can prepare environmentally friendly stability sizing agent (polyamic acid solution) on a large scale and in batches, and the sizing agent prepared at the same time can be applied to various resin-based carbon fiber composite materials. The present invention utilizes the method for preparing sizing agent by water phase, by adding calcium ions to the sizing agent, balancing the hydrogen bond interaction, electrostatic interaction, π-π stacking interaction, cation-π interaction and other supramolecular interactions at the interface of carbon fiber and sizing agent, and improving carbon fiber surface wettability and compatibility.
[0017] The polyamic acid solution and the carbon fiber surface contain a large number of carboxyl groups. Carboxyl groups (-COOH) are chemically substances containing active functional groups, which can participate in a variety of chemical reactions and interactions. The oxygen atoms in the carboxyl group have unshared lone pairs of electrons, which can coordinate with calcium ions to form stable coordination compounds. There are carboxyl groups (-COOH) on the polyamic acid molecular chain, and the oxygen atoms in each carboxyl group can act as ligands to coordinate with calcium ions. When calcium ions approach polyamic acid, their positive charge attracts the negative lone pairs of electrons of the oxygen atoms in the carboxyl group to form a stable calcium-oxygen coordination bond. This process can enhance the interaction between polyamic acid molecules and even promote cross-linking between molecules under certain conditions, thereby changing the physical and chemical properties of the material.
[0018] The carboxyl groups on the surface of carbon fibers can also form coordination bonds with calcium ions through the lone pair of electrons on their oxygen atoms. This coordination effect can not only form a "calcium ion layer" on the surface of carbon fibers, but also provide a bridge for subsequent bonding with polyamic acid or other carboxyl-containing materials, because calcium ions can coordinate with two or more carboxyl groups at the same time to form a cross-linked network structure, thereby enhancing the interaction and bonding strength between the two materials. Through the coordination effect of calcium ions, the carboxyl groups on the surface of polyamic acid and carbon fibers can be effectively "bridged".
[0019] According to the principle of similar compatibility, if the structures of substances are similar, they are easy to dissolve each other or form a stable mixture. In composite materials, the interfacial compatibility between the matrix material and the reinforcing material is crucial to the overall performance of the composite material. Polyimide, as a high-performance resin matrix, has excellent properties such as high temperature resistance, low temperature resistance, high strength and high modulus, high creep resistance, high dimensional stability, low thermal expansion coefficient, and high electrical insulation. And carbon fiber, as a commonly used reinforcing material, also has the characteristics of high strength, high modulus, and high temperature resistance. Using a polyamic acid solution sizing agent to modify carbon fiber, a polyimide coating similar to a polyimide matrix can be formed on the surface of the carbon fiber, thereby enhancing the interfacial compatibility between the carbon fiber and the polyimide matrix. This modification process enables the carbon fiber and the polyimide matrix to form a closer combination at the interface, reducing interface defects and stress concentration phenomena, and improving the overall performance of the composite material. At the same time, since the polyamic acid solution sizing agent has a similar chemical structure to the polyimide matrix, the stability and reliability of the composite material are further enhanced.
[0020] Heat resistance grade is an important indicator for composite materials to maintain performance stability in high temperature environments. As a resin matrix with excellent high temperature resistance, polyimide has a long-term use temperature range of -200 to 300°C, and some of them have no obvious melting point. As a high temperature stable reinforcement material, carbon fiber also has excellent heat resistance. Carbon fiber modified with polyamic acid solution sizing agent can further enhance the interface stability between carbon fiber and polyimide matrix while maintaining its own high temperature stability, thus avoiding interface peeling and performance degradation caused by high temperature.
[0021] The present invention adopts a combination of biphenyl aromatic dianhydride and ether-bonded aromatic diamine. The high rotational freedom brought by the ether bond in the molecular chain drives the molecules to be arranged into regular molecular aggregates through the hydrogen bonding between the end groups, unexpectedly achieving the sp of a large area of polyimide molecular chain segments on the surface of carbon fiber. 2 The molecular assembly under the multi-level structural primitives of the hybrid domain macro-micro interface (such as π-π stacking interaction, cation-π interaction and other long-range forces) increases the surface roughness of the carbon fiber and improves the surface chemical activity. The self-assembled layer forms a modulus transition layer between the carbon fiber and resin interface, transferring the stress concentration point from the carbon fiber surface to the interface phase, so that the interface failure form of the composite material changes from weaker bonding failure to stronger cohesive failure.
[0022] The biphenyl-type aromatic dianhydride and aromatic diamine can ensure that the Tg of the obtained polyimide exceeds 350°C, ensuring high temperature resistance; the introduction of fluorine elements can reduce the surface energy of carbon fiber, making it easier to wet, which helps to improve the mechanical properties of resin-based carbon fiber composites. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The figures are scanning electron microscope images of the carbon fiber tow surface-modified by the sizing agent prepared in the examples and the original carbon fiber tow, a is the example 1, b is the example 2, and c is the original carbon fiber tow;
[0024] Figure 2 This is the infrared image of the surface of carbon fiber precursor;
[0025] Figure 3 This is an infrared image of the surface of carbon fiber filaments surface-modified by the sizing agent prepared in Example 1;
[0026] Figure 4 This is the Raman image of the carbon fiber precursor surface;
[0027] Figure 5 The Raman image of the surface of the carbon fiber filaments surface-modified by the sizing agent prepared in Example 1;
[0028] Figure 6 The XPS graphs of carbon fiber filaments and carbon fiber precursors surface-modified by the sizing agents prepared in Examples 1 and 2 are shown;
[0029] Figure 7 This is the thermal weight loss curve of the sizing agent prepared in Example 1 after thermal imidization reaction;
[0030] Figure 8 Thermal weight loss curve of PI / CF composite material prepared by using carbon fiber surface modified by sizing agent prepared in Example 1;
[0031] Fig. 9 Aging experiment of PI / CF composite material prepared by using carbon fiber surface modified by sizing agent prepared in Examples 1 and 2;
[0032] Fig.10 is a curve showing the relationship between tanδ and temperature of a film prepared using the sizing agent of Example 1;
[0033] Fig.11 The Zeta potential changes of the sizing agent prepared in Example 1 at different settling times. DETAILED DESCRIPTION
[0034] Specific implementation method 1: A high temperature resistant polyimide water-based carbon fiber sizing agent in this implementation method is prepared from triethylamine, aromatic dianhydride, aromatic diamine, deionized water and calcium chloride; the molar ratio of the aromatic dianhydride to the aromatic diamine is 1: (0.9-2); the molar ratio of the aromatic dianhydride to the calcium chloride is 1: (1.9-2.2);
[0035] The aromatic diamine is 4,4'-bis(4-amino-2-trifluoromethylphenoxy)biphenyl or 4,4'-bis(3-aminophenoxy)biphenyl;
[0036] The aromatic dianhydride is 2,2'-difluoromethyl-4,4',5,5'-biphenyltetracarboxylic dianhydride or 3,3',4,4'-biphenyltetracarboxylic dianhydride.
[0037] The structural formula of 4,4'-bis(4-amino-2-trifluoromethylphenoxy)biphenyl described in this specific embodiment is as follows:
[0038]
[0039] The structural formula of 4,4'-bis(3-aminophenoxy)biphenyl described in this specific embodiment is as follows:
[0040]
[0041] The CAS number of 2,2'-difluoromethyl-4,4',5,5'-biphenyltetracarboxylic dianhydride described in this specific embodiment is 165323-75-1, and the structural formula is as follows:
[0042]
[0043] The structural formula of 3,3',4,4'-biphenyltetracarboxylic dianhydride described in this specific embodiment is as follows:
[0044]
[0045] The beneficial effects of this specific implementation are:
[0046] This specific embodiment uses a simple water-phase polycondensation reaction to prepare a high-temperature-resistant water-based sizing agent, which only requires a simple stirring and heating device, and the method process is easy to control and can be used to prepare an environmentally friendly stable sizing agent (polyamic acid solution) on a large scale and in batches. At the same time, the prepared sizing agent can be applied to various resin-based carbon fiber composite materials. This specific embodiment uses a method for preparing a sizing agent in an aqueous phase, and by adding calcium ions to the sizing agent, the hydrogen bond interaction, electrostatic interaction, π-π stacking interaction, cation-π interaction and other supramolecular interactions at the interface between the carbon fiber and the sizing agent are balanced, thereby improving the surface wettability and compatibility of the carbon fiber.
[0047] The polyamic acid solution and the carbon fiber surface contain a large number of carboxyl groups. Carboxyl groups (-COOH) are chemically substances containing active functional groups, which can participate in a variety of chemical reactions and interactions. The oxygen atoms in the carboxyl group have unshared lone pairs of electrons, which can coordinate with calcium ions to form stable coordination compounds. There are carboxyl groups (-COOH) on the polyamic acid molecular chain, and the oxygen atoms in each carboxyl group can act as ligands to coordinate with calcium ions. When calcium ions approach polyamic acid, their positive charge attracts the negative lone pairs of electrons of the oxygen atoms in the carboxyl group to form a stable calcium-oxygen coordination bond. This process can enhance the interaction between polyamic acid molecules and even promote cross-linking between molecules under certain conditions, thereby changing the physical and chemical properties of the material.
[0048] The carboxyl groups on the surface of carbon fibers can also form coordination bonds with calcium ions through the lone pair of electrons on their oxygen atoms. This coordination effect can not only form a "calcium ion layer" on the surface of carbon fibers, but also provide a bridge for subsequent bonding with polyamic acid or other carboxyl-containing materials, because calcium ions can coordinate with two or more carboxyl groups at the same time to form a cross-linked network structure, thereby enhancing the interaction and bonding strength between the two materials. Through the coordination effect of calcium ions, the carboxyl groups on the surface of polyamic acid and carbon fibers can be effectively "bridged".
[0049] According to the principle of similar compatibility, if the structures of substances are similar, they are easy to dissolve each other or form a stable mixture. In composite materials, the interfacial compatibility between the matrix material and the reinforcing material is crucial to the overall performance of the composite material. Polyimide, as a high-performance resin matrix, has excellent properties such as high temperature resistance, low temperature resistance, high strength and high modulus, high creep resistance, high dimensional stability, low thermal expansion coefficient, and high electrical insulation. And carbon fiber, as a commonly used reinforcing material, also has the characteristics of high strength, high modulus, and high temperature resistance. Using a polyamic acid solution sizing agent to modify carbon fiber, a polyimide coating similar to a polyimide matrix can be formed on the surface of the carbon fiber, thereby enhancing the interfacial compatibility between the carbon fiber and the polyimide matrix. This modification process enables the carbon fiber and the polyimide matrix to form a closer combination at the interface, reducing interface defects and stress concentration phenomena, and improving the overall performance of the composite material. At the same time, since the polyamic acid solution sizing agent has a similar chemical structure to the polyimide matrix, the stability and reliability of the composite material are further enhanced.
[0050] Heat resistance grade is an important indicator for composite materials to maintain performance stability in high temperature environments. As a resin matrix with excellent high temperature resistance, polyimide has a long-term use temperature range of -200 to 300°C, and some of them have no obvious melting point. As a high temperature stable reinforcement material, carbon fiber also has excellent heat resistance. Carbon fiber modified with polyamic acid solution sizing agent can further enhance the interface stability between carbon fiber and polyimide matrix while maintaining its own high temperature stability, thus avoiding interface peeling and performance degradation caused by high temperature.
[0051] This specific embodiment uses a combination of biphenyl aromatic dianhydride and ether-bonded aromatic diamine. The high rotational freedom brought by the ether bond in the molecular chain drives the molecules to be arranged into regular molecular aggregates through the hydrogen bonding between the end groups, which unexpectedly achieves the sp of a large area of polyimide molecular chain segments on the surface of carbon fiber. 2 The molecular assembly under the multi-level structural primitives of the hybrid domain macro-micro interface (such as π-π stacking interaction, cation-π interaction and other long-range forces) increases the surface roughness of the carbon fiber and improves the surface chemical activity. The self-assembled layer forms a modulus transition layer between the carbon fiber and resin interface, transferring the stress concentration point from the carbon fiber surface to the interface phase, so that the interface failure form of the composite material changes from weaker bonding failure to stronger cohesive failure.
[0052] The biphenyl-type aromatic dianhydride and aromatic diamine can ensure that the Tg of the obtained polyimide exceeds 350°C, ensuring high temperature resistance; the introduction of fluorine elements can reduce the surface energy of carbon fiber, making it easier to wet, which helps to improve the mechanical properties of resin-based carbon fiber composites.
[0053] Specific embodiment 2: This embodiment is different from specific embodiment 1 in that the molar ratio of the aromatic diamine to triethylamine is 1:(1-2). Other aspects are the same as specific embodiment 1.
[0054] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the mass ratio of the total mass of the aromatic dianhydride and aromatic diamine to the mass ratio of deionized water is 1:(80-99). Other aspects are the same as specific implementation method 1 or 2.
[0055] Specific embodiment 4: This embodiment is a method for preparing a high temperature resistant polyimide water-based carbon fiber sizing agent, which is carried out according to the following steps:
[0056] 1. Weigh triethylamine, aromatic dianhydride, aromatic diamine, deionized water and calcium chloride; the molar ratio of the aromatic dianhydride to the aromatic diamine is 1:(0.9-2); the molar ratio of the aromatic dianhydride to the calcium chloride is 1:(1.9-2.2);
[0057] The aromatic diamine is 4,4'-bis(4-amino-2-trifluoromethylphenoxy)biphenyl or 4,4'-bis(3-aminophenoxy)biphenyl;
[0058] The aromatic dianhydride is 2,2'-difluoromethyl-4,4',5,5'-biphenyltetracarboxylic dianhydride or 3,3',4,4'-biphenyltetracarboxylic dianhydride;
[0059] 2. In a nitrogen atmosphere, at a temperature of 30°C to 35°C and under stirring, triethylamine and aromatic diamine are added to deionized water to react to obtain a reaction solution, the reaction solution is heated to 40°C to 50°C, aromatic dianhydride is added to the reaction solution three times by mass, and the reaction is carried out in a nitrogen atmosphere, at a temperature of 80°C to 85°C and under stirring, and finally calcium chloride is added, and the reaction is carried out in a nitrogen atmosphere, at a temperature of 60°C to 65°C and under stirring to obtain a high temperature resistant polyimide water-based carbon fiber sizing agent.
[0060] Specific embodiment 5: This embodiment is different from specific embodiment 4 in that the molar ratio of the aromatic diamine to triethylamine in step 1 is 1:(1-2). Other aspects are the same as those of specific embodiment 4.
[0061] Specific embodiment 6: This embodiment is different from specific embodiment 4 or 5 in that the mass ratio of the total mass of the aromatic dianhydride and aromatic diamine to the mass ratio of deionized water in step 1 is 1:(80-99). The rest is the same as specific embodiment 4 or 5.
[0062] Specific embodiment 7: This embodiment differs from Specific embodiments 4 to 6 in that: in step 2, under the conditions of nitrogen atmosphere, temperature of 30°C to 35°C and stirring speed of 500rpm to 600rpm, triethylamine and aromatic diamine are added to deionized water for reaction for 0.5h to 1h to obtain a reaction solution. The rest is the same as Specific embodiments 4 to 6.
[0063] Specific embodiment eight: This embodiment differs from specific embodiments four to seven in that: in step two, the reaction liquid is heated to 40°C to 50°C, the aromatic dianhydride is added to the reaction liquid three times by weight, and the reaction is carried out for 1h to 1.5h under the conditions of nitrogen atmosphere, temperature of 80°C to 85°C and stirring speed of 600rpm to 700rpm. The rest is the same as specific embodiments four to seven.
[0064] Specific embodiment 9: This embodiment differs from specific embodiments 4 to 8 in that calcium chloride is added in step 2, and the reaction is carried out for 1 h to 1.5 h under the conditions of nitrogen atmosphere, temperature of 60° C. to 65° C., and stirring speed of 700 rpm to 800 rpm. The rest is the same as specific embodiments 4 to 8.
[0065] Specific embodiment 10: This embodiment differs from specific embodiments 4 to 9 in that: in step 2, triethylamine and aromatic diamine are added to deionized water under nitrogen atmosphere, temperature of 35°C and stirring conditions for 1 hour to obtain a reaction solution, the reaction solution is heated to 50°C, aromatic dianhydride is added to the reaction solution three times by mass, and the reaction is carried out under nitrogen atmosphere, temperature of 80°C and stirring conditions for 1.5 hours, and finally calcium chloride is added, and the reaction is carried out under nitrogen atmosphere, temperature of 60°C and stirring conditions for 1.5 hours. The rest is the same as specific embodiments 4 to 9.
[0066] The following examples are used to verify the beneficial effects of the present invention:
[0067] Embodiment 1:
[0068] A method for preparing a high temperature resistant polyimide water-based carbon fiber sizing agent is carried out according to the following steps:
[0069] 1. Weigh triethylamine, aromatic dianhydride, aromatic diamine, deionized water and calcium chloride; the molar ratio of the aromatic dianhydride to the aromatic diamine is 1:2; the molar ratio of the aromatic dianhydride to the calcium chloride is 1:2; the molar ratio of the aromatic diamine to triethylamine is 1:2; the mass ratio of the total mass of the aromatic dianhydride and the aromatic diamine to the deionized water is 1:99;
[0070] The aromatic diamine is 4,4'-bis(4-amino-2-trifluoromethylphenoxy)biphenyl;
[0071] The aromatic dianhydride is 2,2'-difluoromethyl-4,4',5,5'-biphenyltetracarboxylic dianhydride;
[0072] 2. In a nitrogen atmosphere, a temperature of 35°C and a stirring speed of 500 rpm, triethylamine and aromatic diamine were added to deionized water to react for 1 hour to obtain a reaction solution. The reaction solution was heated to 50°C, and aromatic dianhydride was added to the reaction solution three times by mass, and the reaction was carried out in a nitrogen atmosphere, a temperature of 80°C and a stirring speed of 600 rpm for 1.5 hours. Finally, calcium chloride was added and the reaction was carried out in a nitrogen atmosphere, a temperature of 60°C and a stirring speed of 700 rpm for 1.5 hours to obtain a high temperature resistant polyimide water-based carbon fiber sizing agent.
[0073] Embodiment 2: This embodiment is different from Embodiment 1 in that the aromatic diamine in step 1 is 4,4'-bis(4-amino-2-trifluoromethylphenoxy)biphenyl; the aromatic dianhydride in step 1 is 3,3',4,4'-biphenyltetracarboxylic dianhydride. The rest is the same as Embodiment 1.
[0074] Embodiment 3: This embodiment is different from Embodiment 1 in that the aromatic diamine in step 1 is 4,4'-bis(3-aminophenoxy)biphenyl; the aromatic dianhydride in step 1 is 2,2'-difluoro-3,3',4,4'-biphenyltetracarboxylic dianhydride. The rest is the same as Embodiment 1.
[0075] Embodiment 4: This embodiment is different from Embodiment 1 in that the aromatic diamine in step 1 is 4,4'-bis(3-aminophenoxy)biphenyl and the aromatic dianhydride in step 1 is 3,3',4,4'-biphenyltetracarboxylic dianhydride. The rest is the same as Embodiment 1.
[0076] Comparative Experiment 1: The difference between this comparative experiment and Example 1 is that the aromatic diamine described in step 1 is 4,4'-diaminodiphenyl ether; the aromatic dianhydride described in step 1 is 3,3',4,4'-biphenyltetracarboxylic dianhydride; and calcium chloride is not added in step 2. The rest is the same as Example 1.
[0077] Comparative Experiment 2: The difference between this comparative experiment and Example 1 is that the aromatic diamine described in step 1 is 4,4'-diaminodiphenyl ether; the aromatic dianhydride described in step 1 is 2,2'-bis(3,4-dicarboxylic acid)hexafluoropropane dianhydride; and calcium chloride is not added in step 2. The rest is the same as Example 1.
[0078] Comparative Experiment 3: This comparative experiment is different from Example 1 in that the aromatic diamine described in step 1 is 4,4'-diaminodiphenyl ether; the aromatic dianhydride described in step 1 is 2,2'-bis(3,4-dicarboxylic acid)hexafluoropropane dianhydride. The rest is the same as Example 1.
[0079] (1) Testing of sizing agents:
[0080] 1. The sizing agent prepared in Example 1 was subjected to thermal imidization reaction, and the temperature program was 50°C for 5h, 100°C for 1h, 200°C for 1h, 300°C for 1h, and 400°C for 1h to prepare a film, and the glass transition temperature test was performed: the test was performed using a dynamic mechanical analyzer (DMA). The temperature was raised from room temperature to 450°C, and the heating rate was 5°C / min; the test atmosphere was air.
[0081] 2. The sizing agents prepared in Examples 1 to 4 were subjected to a 3-month static sedimentation experiment at room temperature. At the same time, a nanoparticle size and Zeta potential analyzer (DLS) was used to test the Zeta potential changes of the sizing agent solutions in Example 1 at different static sedimentation times.
[0082] (ii) Testing of single carbon fiber yarn and carbon fiber precursor on carbon fiber tows surface modified by sizing agent and original carbon fiber tows:
[0083] The carbon fiber tow (Toray T300B-1000 desizing with acetone) was sizing treated with the sizing agent prepared in Examples 1 to 4 and Comparative Experiments 1 to 3, dried in a vacuum drying oven at 80°C for 1 hour, and then subjected to imidization treatment by programmed temperature increase: 100°C for 1 hour, 200°C for 1 hour, 300°C for 1 hour, and 400°C for 1 hour. Finally, the modified carbon fiber tow was rolled up for use to obtain a carbon fiber tow with a surface modified by the sizing agent; the mass ratio of the carbon fiber tow with a surface modified by the sizing agent to the untreated carbon fiber tow was 1.02:1.
[0084] At the same time, according to the process of Example 3 in the patent publication number CN105461926A "An environmentally friendly stable polyamide acid solution and its preparation method", a prepreg with a solid mass percentage of 16% was prepared, and the aromatic dianhydride used was 3,3',4,4'-biphenyltetracarboxylic dianhydride, and the aromatic diamine was p-phenylenediamine.
[0085] 3. Use dynamic contact angles (DCA) to evaluate the dynamic contact angles between carbon fiber monofilaments and deionized water before and after treatment. This experiment uses the DCAT 21 surface / interfacial tension analyzer from DataPhysics Instruments of Germany to test a series of carbon fibers. During the test, a 50mm×10mm rectangular cardboard fixture was used to fix the carbon fiber. Four carbon fiber monofilament samples were pasted on each test specimen at a parallel interval of 2mm. The fiber length outside the fixture was kept at 6mm, the threshold of the carbon fiber insertion depth was set to 4mm, the fiber infiltration speed was 0.1mm / s, the detection mass threshold was set to 0.08mg, and the test speeds of the advancing angle and the receding angle were set to 0.08mm / s. The contact angles of the carbon fiber and the liquid were measured respectively.
[0086] 4. Single fiber tensile properties: A single fiber strength tester with a heating platform was used to test the tensile strength, tensile modulus and elongation at break of single fiber at room temperature and 300°C; the test sensor range, gauge length and speed were 0-5N, 200mm and 1mm / min respectively. At least 30 specimens were tested for each system, and the Weibull method was used to perform statistical analysis on the data.
[0087] 5. High and low temperature shear effect between two fibers: Under an optical microscope, the carbon fiber monofilaments modified by different sizing agents were overlapped with an overlap length of 10 mm, and the prepreg with a solid mass percentage of 16% prepared above was evenly applied on the overlap. The curing was carried out according to the following processes: 50℃ / 5h, 100℃ / 0.5h, 200℃ / 1h, 300℃ / 1h, 300℃ / 1h, 400℃ / 1h, and then the shear tensile strength under different temperature conditions was simulated, and the overlap length and overlap area were recorded. The shear force was tested with a single fiber strength tester at room temperature and 300℃. The test speed was 0.1mm / min, and the shear strength was calculated. At least 30 specimens were tested for each system.
[0088] 6. Use a single fiber strength tester to coat the carbon fiber monofilaments before and after modification into the prepreg prepared above with a solid mass percentage of 16%. The heat treatment process is 50℃ / 6h, 100℃ / 1h, 200℃ / 1h, 300℃ / 1h, and 400℃ / 1h. Use sandpaper to carefully smooth it, measure the thickness of the coating resin, and use a single fiber strength tester to perform a single fiber pull-out test at room temperature and 300℃. The test rate is 0.1mm / min, and at least 30 samples are tested for each system. Calculate the single fiber interfacial shear strength (IFSS).
[0089] 7. The changes in the physical and chemical properties of the carbon fiber surface before and after modification are characterized by Fourier transform infrared spectroscopy, X-ray photoelectron spectroscopy and Raman spectroscopy.
[0090] (III) Preparation of polyimide continuous carbon fiber reinforced composite materials by solution impregnation method and testing:
[0091] The specific preparation process is as follows: ① Cut the unidirectional continuous carbon fiber tow longitudinally (vertical to the axis), and arrange the carbon fiber tow modified by the sizing agent surface in parallel; ② Put the parallel arranged and sizing agent surface modified carbon fiber tow into the above-prepared prepreg with a solid mass percentage of 16% to fully wet it, then take it out, let it stand at room temperature for one day to eliminate bubbles, and then put it in a 90°C oven to dry the solvent; ③ Cut it according to the required size, stack 8 prepregs in a [0° / 90°]4 stacking manner in the mold, and then put it into a hot press, and then program the temperature: 100°C 1h, 200°C 1h, 300°C 1h, 400°C 1h for imidization treatment, and at the same time discharge excess gas in the mold to reduce the porosity in the composite material. The pressure of this process is 50Kgf / cm 2 After natural cooling, a PI / CF composite material was obtained; the content of resin in the PI / CF composite material was calculated by the thermogravimetric method, and the mass ratio of resin to carbon fiber was about 3:7.
[0092] 8. The PI / CF composite material was cut into composite material specimens with a size of 40mm×20mm×4mm (the mass percentage of carbon fiber is 70%), and the shear strength ILSS of the composite material was tested by a universal material testing machine in accordance with GB / T 3375 standard, and the load-displacement curve performance was recorded; the PI / CF composite material was cut into TFBT specimens with a size of 100mm×20mm×3mm, and the tensile strength of the composite material was tested by a universal material testing machine with reference to GB / T 2567-2008 standard, and the load-displacement curve was recorded; the PI / CF composite material was cut into composite material specimens with a size of 60mm×20mm×4mm, and the flexural strength (Flexural Strength) of the composite material was tested by a universal material testing machine with reference to GB / T 41762.2-2022 standard, and the load-displacement curve performance was recorded; the tensile strength, flexural strength and interlaminar shear strength of the composite material were tested at room temperature and 300°C using a universal material testing machine with a heating table.
[0093] 9. The sizing agent prepared in Example 1 was subjected to thermal imidization reaction with a temperature program of 50°C for 5 h, 100°C for 1 h, 200°C for 1 h, 300°C for 1 h, and 400°C for 1 h to obtain a cured sizing agent. The cured sizing agent and the PI / CF composite material were subjected to thermal gravimetric test.
[0094] 10. The Tg of the composite material determines the maximum use temperature of the material, and Tg is mainly affected by the resin matrix. In order to study the effect of aging test on the use temperature of the composite material, the peak value of tanδ is used as the glass transition temperature. After the PI / CF composite material was aged at 300℃ for different times (aging time was 0h, 100h, 200h, 300h, 400h, 500h, 600h), the composite material was tested by DMA.
[0095] Table 1
[0096]
[0097]
[0098] Figure 1 The scanning electron microscope images of the carbon fiber tow surface modified by the sizing agent prepared in the examples and the original carbon fiber tow, a is the example 1, b is the example 2, and c is the original carbon fiber tow; it can be seen from the figure that the surface of the carbon fiber precursor has obvious grooves distributed along the axial direction, which has typical fiber structure characteristics. Figures a and b are the microscopic morphology of the carbon fiber surface after sizing, and a large area of sp 2 Under the action of the hybrid domain, it spontaneously assembles into a three-dimensional macroscopic ordered structure, increases the surface roughness of the carbon fiber, and enhances the mechanical meshing effect between the fiber and the matrix.
[0099] Figure 2 This is the infrared image of the surface of carbon fiber precursor; Figure 3 This is an infrared image of the surface of the carbon fiber modified by the sizing agent prepared in Example 1. As can be seen from the figure, the carbon fiber raw fiber shows no characteristic peak absorption, while the surface of the carbon fiber modified by sizing shows 1770-1784cm -1 (C=O asymmetric stretching vibration), 1705-1720cm -1 (C=O symmetric stretching vibration) and 1350-1370cm -1 The characteristic absorption peak of polyimide at (CN stretching vibration) proves the successful synthesis of polyimide.
[0100] Figure 4 This is the Raman image of the carbon fiber precursor surface; Figure 5 This is the Raman spectrum of the surface of the carbon fiber modified by the sizing agent prepared in Example 1. As can be seen from the figure, compared with the Raman spectrum of the carbon fiber precursor, the D and G peaks of the carbon fiber treated in Example 1 have interference background, which comes from the interference of the benzene ring fluorescence in the sizing agent. At the same time, the G peak of the carbon fiber treated by sizing is compared with the G peak of the carbon fiber precursor (1586.79cm -1 ) frequency shifted to 1594.75cm -1 , attributed to the benzene ring and the carbon fiber surface sp 2 π-π interaction of hybrid domains.
[0101] Figure 6 The XPS graphs of carbon fiber filaments and carbon fiber precursors surface-modified by the sizing agent prepared in Examples 1 and 2 are shown in the figure. As can be seen from the figure, there is little or no N element on the surface of the carbon fiber precursor. After the surface modification by the sizing agent, N and F elements appear on the surface of the carbon fiber, which can significantly increase the surface activity of the carbon fiber and improve the wettability to the resin matrix.
[0102] Figure 7 This is the thermal weight loss curve of the sizing agent prepared in Example 1 after thermal imidization reaction; Figure 8 Thermal weight loss curve of PI / CF composite material prepared by using carbon fiber surface modified by sizing agent prepared in Example 1; As can be seen from the figure, the thermal weight loss T 5% All above 500℃, showing good high temperature resistance
[0103] Fig. 9 Aging experiment of PI / CF composite material prepared by using carbon fiber surface modified by sizing agent prepared in Examples 1 and 2; as can be seen from the figure, after aging for 600h, Tg is stable at above 350°C, still showing excellent high temperature resistance.
[0104] Fig.10The curve of the relationship between tanδ and temperature of the film prepared by using the sizing agent of Example 1; it can be seen from the figure that the Tg of the prepared polyimide is as high as 400°C.
[0105] The sizing agents prepared in Examples 1 to 4 were subjected to a three-month static sedimentation test at room temperature. No stratification or aggregation was found by visual observation, and the sizing agents showed good stability. Fig.11 The Zeta potential change of the sizing agent prepared in Example 1 at different settling times; it can be seen from the figure that the Zeta potential value can be stabilized at -30mV after 10 days, indicating that the prepared sizing agent has good stability.
Claims
1. A high temperature resistant polyimide water-based carbon fiber sizing agent, characterized in that It is prepared from triethylamine, aromatic dianhydride, aromatic diamine, deionized water and calcium chloride; the molar ratio of the aromatic dianhydride to the aromatic diamine is 1:(0.9-2); the molar ratio of the aromatic dianhydride to the calcium chloride is 1:(1.9-2.2); The aromatic diamine is 4,4'-bis(4-amino-2-trifluoromethylphenoxy)biphenyl or 4,4'-bis(3-aminophenoxy)biphenyl; The aromatic dianhydride is 2,2'-difluoromethyl-4,4',5,5'-biphenyltetracarboxylic dianhydride or 3,3',4,4'-biphenyltetracarboxylic dianhydride.
2. A high temperature resistant polyimide water-based carbon fiber sizing agent according to claim 1, characterized in that The molar ratio of the aromatic diamine to triethylamine is 1:(1-2).
3. A high temperature resistant polyimide water-based carbon fiber sizing agent according to claim 1, characterized in that The mass ratio of the total mass of the aromatic dianhydride and the aromatic diamine to the deionized water is 1:(80-99).
4. The method for preparing a high temperature resistant polyimide water-based carbon fiber sizing agent according to claim 1, characterized in that It is carried out in the following steps:
1. Weigh triethylamine, aromatic dianhydride, aromatic diamine, deionized water and calcium chloride; the molar ratio of the aromatic dianhydride to the aromatic diamine is 1:(0.9-2); the molar ratio of the aromatic dianhydride to the calcium chloride is 1:(1.9-2.2); The aromatic diamine is 4,4'-bis(4-amino-2-trifluoromethylphenoxy)biphenyl or 4,4'-bis(3-aminophenoxy)biphenyl; The aromatic dianhydride is 2,2'-difluoromethyl-4,4',5,5'-biphenyltetracarboxylic dianhydride or 3,3',4,4'-biphenyltetracarboxylic dianhydride; 2. In a nitrogen atmosphere, at a temperature of 30°C to 35°C and under stirring, triethylamine and aromatic diamine are added to deionized water to react to obtain a reaction solution, the reaction solution is heated to 40°C to 50°C, aromatic dianhydride is added to the reaction solution three times by mass, and the reaction is carried out in a nitrogen atmosphere, at a temperature of 80°C to 85°C and under stirring, and finally calcium chloride is added, and the reaction is carried out in a nitrogen atmosphere, at a temperature of 60°C to 65°C and under stirring to obtain a high temperature resistant polyimide water-based carbon fiber sizing agent.
5. The method for preparing a high temperature resistant polyimide water-based carbon fiber sizing agent according to claim 4, characterized in that The molar ratio of the aromatic diamine to triethylamine in step 1 is 1:(1-2).
6. The method for preparing a high temperature resistant polyimide water-based carbon fiber sizing agent according to claim 4, characterized in that The mass ratio of the total mass of the aromatic dianhydride and the aromatic diamine described in step 1 to deionized water is 1:(80-99).
7. The method for preparing a high temperature resistant polyimide water-based carbon fiber sizing agent according to claim 4, characterized in that In step 2, under the conditions of nitrogen atmosphere, temperature of 30° C. to 35° C. and stirring speed of 500 rpm to 600 rpm, triethylamine and aromatic diamine are added to deionized water for reaction for 0.5 h to 1 h to obtain a reaction solution.
8. The method for preparing a high temperature resistant polyimide water-based carbon fiber sizing agent according to claim 4, characterized in that In step 2, the reaction solution is heated to 40°C to 50°C, and the aromatic dianhydride is added to the reaction solution three times by weight, and the reaction is carried out for 1h to 1.5h under the conditions of nitrogen atmosphere, temperature of 80°C to 85°C and stirring speed of 600rpm to 700rpm.
9. The method for preparing a high temperature resistant polyimide water-based carbon fiber sizing agent according to claim 4, characterized in that In step 2, calcium chloride is added and the reaction is carried out for 1 h to 1.5 h under the conditions of nitrogen atmosphere, temperature of 60° C. to 65° C. and stirring speed of 700 rpm to 800 rpm.
10. The method for preparing a high temperature resistant polyimide water-based carbon fiber sizing agent according to claim 4, characterized in that In step 2, triethylamine and aromatic diamine are added to deionized water under nitrogen atmosphere, temperature of 35°C and stirring conditions, and the reaction is carried out for 1 hour to obtain a reaction solution. The reaction solution is heated to 50°C, and aromatic dianhydride is added to the reaction solution three times by mass, and the reaction is carried out under nitrogen atmosphere, temperature of 80°C and stirring conditions for 1.5 hours. Finally, calcium chloride is added, and the reaction is carried out under nitrogen atmosphere, temperature of 60°C and stirring conditions for 1.5 hours.
Citation Information
Cited By
Sizing agent for quartz fiber as well as preparation method and application of sizing agent
CN121407396A
High-temperature-resistant water-based sizing agent as well as preparation method and application thereof
CN121735795A