Method for optimizing adhesiveness of PEDOT: PSS conductive film based on solution doping modification
By doping PVA, ethanol and DMSO into the PEDOT:PSS conductive polymer material, combined with ultrasonic cleaning and spin coating technology, the problem of insufficient adhesion of PEDOT:PSS was solved, and the adhesion and film-forming quality of the film were significantly improved. It is suitable for Based on a variety of base materials, it expands its application in complex environments.
Patent Information
- Application Number
- CN202410859186.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-01
AI Technical Summary
PEDOT:PSS conductive polymer materials have poor adhesion in practical applications and are easy to peel or separate, affecting the reliability and stability of the device.
It adopts a process of doping polyvinyl alcohol (PVA), ethanol and dimethyl sulfoxide (DMSO) with PEDOT:PSS solution, and improves the adhesion of PEDOT:PSS film through ultrasonic cleaning and spin coating technology. It is suitable for quartz wafers, silicon sheet and polyvinylidene fluoride (PVDF) substrate.
The film-forming rate and film-forming quality of the PEDOT:PSS film are significantly improved. It is easy to operate, low-cost, and has a mature process. It is suitable for biosensors, wearable devices and other fields to ensure the reliability and stability of the device in complex environments.
Smart Images

Figure CN118737565A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electronic component manufacturing, and in particular is a method for optimizing the adhesion of a PEDOT:PSS conductive film based on solution doping modification. Background Art
[0002] (1) Conductive polymers are a class of materials that have the advantages of being easy to use, easy to process, and having controllable conductivity and corrosion resistance. In recent years, poly(3,4-ethylenedioxythiophene) / poly(p-styrene sulfonic acid) (PEDOT:PSS) has attracted extensive attention as a typical conductive polymer material. PEDOT:PSS has the characteristics of high conductivity (after doping), high light transmittance, excellent environmental stability, and solution processability, making it a widely used conductive polymer material. It is used in the field of organic optoelectronic devices, including organic solar cells, organic field effect transistors, and organic light-emitting diodes.
[0003] (2) However, in practical applications, the adhesion of PEDOT:PSS to the substrate is often not ideal, and it is prone to peeling, separation, or loose structure. In order to improve the adhesion of PEDOT:PSS solution, researchers have been working hard to enhance the adhesion between PEDOT:PSS and the substrate to improve the reliability and stability of the material in device preparation.
[0004] (3) Existing technologies for improving the adhesion of PEDOT:PSS films can be divided into two categories: substrate treatment and solution treatment. Substrate treatment technologies can be specifically divided into two types, namely surface treatment: chemical or physical treatment of the substrate surface, such as plasma water cleaning, UV light, oxide film coating, etc., can improve the roughness and chemical affinity of the substrate surface and enhance the adhesion between the PEDOT:PSS film and the substrate; doping the substrate surface: introducing a covering layer on the substrate surface, such as a polymer or functionalized molecule, to interact with PEDOT:PSS and improve adhesion. The advantage of this type of technology is that it directly affects the adhesion of the PEDOT:PSS film by improving the physical and chemical properties of the substrate surface, is relatively stable, and is not easily affected by changes in solution composition. However, the preparation process is relatively complex, requires complicated processing steps, has restrictions on substrate materials, and is not suitable for all types of substrates. Solution processing technology is usually solution doping, which improves the hydrophilicity and flow properties of the solution and the flatness and adhesion of the PEDOT:PSS film by adding reagents such as ethanol and propylene glycol to the PEDOT:PSSS solution, or adds surfactants such as Triton to improve the surface tension and contact angle of the solution and improve the adhesion of the PEDOT:PSS film. The advantage of this technology is that it can improve the adhesion by directly changing the composition of the PEDOT:PSS solution. It has a wide range of applications, simple operation and short process. However, the existing technologies use a large number of doping solutions, and the ratio also needs to be precisely controlled. Too high or too low doping ratios will affect the performance of the PEDOT:PSS film. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art, and propose a method for optimizing the adhesion of PEDOT:PSS conductive film based on solution doping modification, which uses a process of doping polyvinyl alcohol (PVA), ethanol, dimethyl sulfoxide (DMSO) with PEDOT:PSS solution to effectively improve the adhesion of PEDOT:PSS film on quartz wafers, silicon wafers, and polyvinylidene fluoride (PVDF) substrates, greatly improving the film formation rate and film quality, and is easy to operate, low in cost, mature in process, and high in success rate. Improving the adhesion of PEDOT:PSS can expand its application in various fields, including biosensors, wearable devices, smart textiles, etc. These fields have higher requirements for stable PEDOT:PSS film adhesion to ensure the reliability and stability of the device in complex environments.
[0006] The present invention solves the technical problem by adopting the following technical solutions:
[0007] A method for optimizing the adhesion of a PEDOT:PSS conductive film based on solution doping modification comprises the following steps:
[0008] Step 1: Clean the substrate using an ultrasonic cleaner and blow dry with nitrogen;
[0009] Step 2, doping the PEDOT:PSS solution with the DMSO solution;
[0010] Step 3, preparing PVA solution;
[0011] Step 4, doping the PEDOT:PSS solution doped with DMSO in step 2 with the ethanol solution and the PVA solution prepared in step 3 respectively;
[0012] Step 5, spin coating the ethanol-doped and PVA-doped PEDOT:PSS solutions in step 4 on the substrate using a coating machine;
[0013] Step 6: Place the spin-coated substrate on a hot plate for heating to obtain a stable PEDOT:PSS conductive film.
[0014] Moreover, the specific implementation method of using an ultrasonic cleaning machine to clean the substrate in step 1 is: ultrasonic cleaning is carried out in deionized water, ethanol and isopropanol in this order for 10 minutes.
[0015] Moreover, the specific implementation method of step 2 is to dope the PEDOT:PSS solution and the DMSO solution in a volume ratio ranging from 100:5 to 100:15.
[0016] Moreover, the mass percentage of PVA in step 3 is 3% to 9%.
[0017] Moreover, in the step 4, the volume ratio of the PEDOT:PSS solution doped with DMSO to the ethanol solution is 1:1 to 10:1; the volume ratio of the PEDOT:PSS solution doped with DMSO to the PVA solution is 1:1 to 15:1.
[0018] Moreover, during the spin coating in step 5, the rotation speed of the coating machine is between 1500 rpm and 6000 rpm, and the spin coating time is 20 to 50 s.
[0019] Moreover, the specific implementation method of step 6 is: placing the spin-coated substrate on a hot plate and heating it at 90° C. for 10 minutes to obtain a stable PEDOT:PSS conductive film.
[0020] The advantages and positive effects of the present invention are:
[0021] 1. The present invention utilizes a process of doping polyvinyl alcohol (PVA), ethanol, dimethyl sulfoxide (DMSO) with a PEDOT:PSS solution, which can effectively improve the adhesion of PEDOT:PSS films on quartz wafers, silicon wafers, and polyvinylidene fluoride (PVDF) substrates, greatly improving the film formation rate and film quality, and is easy to operate, low in cost, mature in process, and high in success rate. Improving the adhesion of PEDOT:PSS can expand its application in various fields, including biosensors, wearable devices, smart textiles, etc. These fields have higher requirements for stable PEDOT:PSS film adhesion to ensure the reliability and stability of the device in complex environments.
[0022] 2. The method for improving the adhesion of PEDOT:PSS film provided by the present invention adopts a solution doping process, which has a simple process, a short cycle, low cost and a high success rate.
[0023] 3. During the configuration process, the present invention is effective when the volume ratio of PEDOT:PSS solution to PVA solution is 1:1 to 15:1, and when the volume ratio of PEDOT:PSS solution to ethanol solution is 1:1 to 10:1.
[0024] 4. The present invention has a significant effect on improving the adhesion of PEDOT:PSS thin films. The doping of PEDOT:PSS solution and PVA solution can form a film on a hydrophobic material. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a film formation diagram of PEDOT:PSS on a quartz substrate after doping with ethanol in Example 1 of the present invention.
[0026] Figure 2 This is a film formation diagram of PEDOT:PSS on a quartz substrate after doping with PVA in Example 1 of the present invention.
[0027] Figure 3 This is a film formation diagram of PEDOT:PSS on a silicon wafer substrate after doping with ethanol in Example 2 of the present invention.
[0028] Figure 4 This is a film formation diagram of PEDOT:PSS on a silicon wafer substrate after doping with PVA in Example 2 of the present invention.
[0029] Figure 5 This is a film formation diagram of PEDOT:PSS on a PVDF substrate after doping with ethanol in Example 3 of the present invention.
[0030] Figure 6 This is a film formation diagram of PEDOT:PSS on a PVDF substrate after doping with PVA in Example 3 of the present invention.
[0031] (In all the above figures, the first row is the substrate without film formation as a blank control, the second row is the undoped PEDOT:PSS film formation, and the third to fifth rows are the film formation effect diagrams after doping) DETAILED DESCRIPTION
[0032] The present invention is further described in detail below with reference to the accompanying drawings.
[0033] A method for optimizing the adhesion of a PEDOTPSS conductive film based on solution doping modification comprises the following steps:
[0034] Step 1: Clean the substrate using an ultrasonic cleaner and blow dry with nitrogen.
[0035] The specific implementation method of using an ultrasonic cleaning machine to clean the substrate is as follows: ultrasonic cleaning is performed in deionized water, ethanol and isopropanol in this order for 10 minutes.
[0036] Step 2: PEDOT:PSS solution and DMSO solution are doped in a volume ratio ranging from 100:5 to 100:15.
[0037] Step 3: prepare a PVA solution, wherein the mass percentage of PVA is 3% to 9%.
[0038] Step 4: doping the PEDOT:PSS solution doped with DMSO in step 2 with the ethanol solution and the PVA solution prepared in step 3 respectively.
[0039] The volume ratio of the PEDOT:PSS solution doped with DMSO to the ethanol solution is 1:1 to 10:1; the volume ratio of the PEDOT:PSS solution doped with DMSO to the PVA solution is 1:1 to 15:1
[0040] Step 5: Spin-coat the ethanol-doped and PVA-doped PEDOT:PSS solutions in step 4 on the substrate using a coating machine, respectively. The rotation speed of the coating machine is between 1500 rpm and 6000 rpm, and the coating time is 20 to 50 s.
[0041] Step 6: Place the spin-coated substrate on a hot plate and heat at 90° C. for 10 min to obtain a stable PEDOT:PSS conductive film.
[0042] According to the above-mentioned method for optimizing the adhesion of PEDOTPSS conductive film based on solution doping modification, multiple tests were performed to verify the effect of the present invention.
[0043] Example 1
[0044] A method for optimizing the adhesion of PEDOT:PSS conductive films based on solution doping modification:
[0045] (1) Clean a 2 cm × 2 cm quartz plate by ultrasonic oscillation in deionized water, ethanol, and isopropanol for 10 min in that order, and blow dry with nitrogen for later use;
[0046] (2) PEDOT:PSS solution and DMSO solution were mixed in a volume ratio of 100:15;
[0047] (3) preparing a PVA solution, wherein the mass percentage of PVA is 8%;
[0048] (4) doping the PEDOT:PSS solution doped with DMSO with a PVA solution in a volume ratio of 3:1, 5:1, and 8:1, and doping the PEDOT:PSS solution doped with DMSO with an ethanol solution in a volume ratio of 3:1, 5:1, and 8:1;
[0049] (5) Spin coating the ethanol-doped and PVA-doped PEDOT:PSS solutions on the substrate using a spin coater, respectively, with the spin coater rotating at a speed between 3000 rpm and 4000 rpm and the spin coating time being 20 to 40 s;
[0050] (6) Spin coating a PEDOT:PSS solution doped with only DMSO on a quartz substrate using a spin coater as a control, with the spin coater speed being between 3000 rpm and 4000 rpm and the spin coating time being between 20 and 40 s;
[0051] (7) The substrate formed by spin coating was placed on a hot plate and heated at 90°C for 10 min to obtain a stable PEDOT:PSS conductive film. Figure 1 and Figure 2 shown.
[0052] Depend on Figure 1 Figure 2 It can be seen that the PEDOT:PSS solution doped with DMSO alone has poor film-forming properties on the quartz substrate, and the film surface is extremely uneven with significant lines. After doping with PVA or ethanol, the film adhesion is improved, the film is smooth, and almost no lines are produced. Comparing the effect diagrams of the two doping methods, it can be seen that PVA doping has a better effect.
[0053] Example 2
[0054] A method for optimizing the adhesion of PEDOT:PSS conductive films based on solution doping modification:
[0055] (1) Cut the silicon wafer into pieces of 1.5 cm × 1.5 cm to 2 cm × 2 cm, clean them in deionized water, ethanol, and isopropanol in this order by ultrasonic oscillation for 10 min, and blow dry them with nitrogen for later use;
[0056] (2) PEDOT:PSS solution and DMSO solution were mixed in a volume ratio of 100:15;
[0057] (3) preparing a PVA solution, wherein the mass percentage of PVA is 8%;
[0058] (4) doping the PEDOT:PSS solution doped with DMSO with a PVA solution in a volume ratio of 3:1, 5:1, and 8:1, and doping the PEDOT:PSS solution doped with DMSO with an ethanol solution in a volume ratio of 3:1, 5:1, and 8:1;
[0059] (5) Spin coating the ethanol-doped and PVA-doped PEDOT:PSS solutions on the substrate using a spin coater, respectively, with the spin coater rotating at a speed between 3000 rpm and 4000 rpm and the spin coating time being 20 to 40 s;
[0060] (6) Spin coating a PEDOT:PSS solution doped with only DMSO on a quartz substrate using a spin coater as a control, with the spin coater speed being between 3000 rpm and 4000 rpm and the spin coating time being between 20 and 40 s;
[0061] (7) The substrate formed by spin coating was placed on a hot plate and heated at 90°C for 10 min to obtain a stable PEDOT:PSS conductive film. Figure 3 and Figure 4 shown.
[0062] Depend on Figure 3 Figure 4 It can be seen that the film-forming effect of the PEDOT:PSS solution doped with only DMSO on the silicon wafer substrate is worse than that on the quartz wafer. Due to insufficient adhesion, the film-forming area on the silicon wafer is even less than one-half, and the surface of the film-forming part is not uniform enough, with obvious textures. After doping with PVA or ethanol, the film adhesion is significantly improved, which can ensure basic film-forming properties and a larger film-forming area. By comparing the effect diagrams of the two doping methods of PVA and ethanol, it can be found that the film is smoother, the surface is more uniform, and the effect is better after PVA doping.
[0063] Example 3
[0064] A method for optimizing the adhesion of PEDOT:PSS conductive films based on solution doping modification:
[0065] (1) Cut PVDF into sheets of 1.5 cm × 1.5 cm to 2 cm × 2 cm, clean them in deionized water, ethanol, and isopropanol in this order by ultrasonic oscillation for 10 min, and blow dry them with nitrogen for later use;
[0066] (2) PEDOT:PSS solution and DMSO solution were mixed in a volume ratio of 100:15;
[0067] (3) preparing a PVA solution, wherein the mass percentage of PVA is 8%;
[0068] (4) doping the PEDOT:PSS solution doped with DMSO with a PVA solution in a volume ratio of 3:1, 5:1, and 8:1, and doping the PEDOT:PSS solution doped with DMSO with an ethanol solution in a volume ratio of 3:1, 5:1, and 8:1;
[0069] (5) Spin coating the ethanol-doped and PVA-doped PEDOT:PSS solutions on the substrate using a spin coater, respectively, with the spin coater rotating at a speed between 3000 rpm and 4000 rpm and the spin coating time being 20 to 40 s;
[0070] (6) Spin coating a PEDOT:PSS solution doped with only DMSO on a quartz substrate using a spin coater as a control, with the spin coater speed being between 3000 rpm and 4000 rpm and the spin coating time being between 20 and 40 s;
[0071] (7) The substrate formed by spin coating was placed on a hot plate and heated at 90°C for 10 min to obtain a stable PEDOT:PSS conductive film. Figure 5 , Figure 6 .
[0072] Depend on Figure 5 Figure 6 It can be seen that since PVDF is a highly hydrophobic material, it is much more difficult to form a film on its surface. Undoped PEDOT:PSS solution, PEDOT:PSS solution doped with DMSO only, and PEDOT:PSS solution doped with DMSO and ethanol cannot form a film on the PVDF surface. Figure 6 As shown in the figure, the PVA-doped PEDOT:PSS solution can form a film on the PVDF hydrophobic material, and the film-forming effect is good, indicating that compared with ethanol doping, PVA doping has a more significant improvement in film adhesion. And when the PVDF is bent, the surface film will not peel off or crack due to deformation, indicating that PVA doping can improve the flexibility and strength of the PEDOT:PSS film, making it adaptable to various deformations and stresses.
[0073] It should be emphasized that the embodiments described in the present invention are illustrative rather than restrictive. Therefore, the present invention includes but is not limited to the embodiments described in the specific implementation manner. Any other implementation manners derived by those skilled in the art based on the technical solution of the present invention also fall within the scope of protection of the present invention.
Claims
1. A method for optimizing the adhesion of a PEDOT:PSS conductive film based on solution doping modification, characterized in that: The following steps are involved: Step 1: Clean the substrate using an ultrasonic cleaner and blow dry with nitrogen; Step 2, doping the PEDOT:PSS solution with the DMSO solution; Step 3, preparing PVA solution; Step 4, doping the PEDOT:PSS solution doped with DMSO in step 2 with the ethanol solution and the PVA solution prepared in step 3 respectively; Step 5, spin coating the ethanol-doped and PVA-doped PEDOT:PSS solutions in step 4 on the substrate using a coating machine; Step 6: Place the spin-coated substrate on a hot plate for heating to obtain a stable PEDOT:PSS conductive film.
2. The method for optimizing the adhesion of a PEDOTPSS conductive film based on solution doping modification according to claim 1, characterized in that: The specific implementation method of using an ultrasonic cleaning machine to clean the substrate in step 1 is: ultrasonic cleaning is carried out in deionized water, ethanol and isopropanol in this order for 10 minutes.
3. The method for optimizing adhesion of PEDOTPSS conductive film based on solution doping modification according to claim 1, characterized in that: The specific implementation method of step 2 is to mix and dope the PEDOT:PSS solution and the DMSO solution in a volume ratio ranging from 100:5 to 100:
15.
4. The method for optimizing adhesion of a PEDOT:PSS conductive film based on solution doping modification according to claim 1, characterized in that: The mass percentage of PVA in step 3 is in the range of 3% to 9%.
5. The method for optimizing adhesion of PEDOTPSS conductive film based on solution doping modification according to claim 1, characterized in that: In the step 4, the volume ratio of the PEDOT:PSS solution doped with DMSO to the ethanol solution is in the range of 1:1 to 10:1; the volume ratio of the PEDOT:PSS solution doped with DMSO to the PVA solution is in the range of 1:1 to 15:
1.
6. The method for optimizing adhesion of PEDOTPSS conductive film based on solution doping modification according to claim 1, characterized in that: During the spin coating in step 5, the rotation speed of the coating machine is between 1500 rpm and 6000 rpm, and the spin coating time is 20 to 50 seconds.
7. The method for optimizing the adhesion of a PEDOT:PSS conductive film based on solution doping modification according to claim 1, characterized in that: The specific implementation method of step 6 is: placing the spin-coated substrate on a hot plate and heating it at 90° C. for 10 minutes to obtain a stable PEDOT:PSS conductive film.