Negative electrode mixture, negative electrode, and secondary battery
By using a negative electrode mixture of single-layer carbon nanotubes and fluorine-containing copolymers in secondary batteries, a strong and tightly bonded structure with the metal foil electrode is formed, which solves the problem of battery performance degradation caused by the expansion and contraction of the negative electrode, improves cycle characteristics and reduces battery life. The gas increase rate is significantly improved, which significantly improves the stability and performance of the battery.
Patent Information
- Application Number
- CN202380016651.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-17
- Filing Date
- 2023-01-06
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing secondary battery anode materials expand and contract during the charge and discharge process, resulting in battery performance degradation, and the gas increase rate is high after repeated charge and discharge, affecting cycle characteristics.
Using a negative electrode mixture containing single-layer carbon nanotubes and fluorine-containing copolymers, the single-layer carbon nanotubes form a three-dimensional network structure that is extremely firmly adhered to the metal foil. The fluorine-containing copolymer is used to improve flexibility and adhesion, and reduce expansion and contraction. Impact on battery performance.
The anode material layer with excellent flexibility is realized, which improves the battery's cycle characteristics and gas increase rate after repeated charge and discharge, and significantly improves the stability and performance of the battery.
Smart Images

Figure BDA0004934658950000061 
Figure BDA0004934658950000161 
Figure BDA0004934658950000231
Abstract
Description
Technical Field
[0001] The present invention relates to a negative electrode mixture, a negative electrode, and a secondary battery. Background Art
[0002] Patent Document 1 describes a secondary battery including a positive electrode, a negative electrode, and an electrolytic solution. The negative electrode includes a first negative electrode active material, a second negative electrode active material, and a negative electrode binder. The first negative electrode active material includes a central portion containing a material containing silicon (Si) as a constituent element, and a coating portion provided on the surface of the central portion and containing a salt compound and a conductive material. The salt compound contains at least one of polyacrylate and carboxymethylcellulose salt, and the conductive material contains at least one of a carbon material and a metal material. The second negative electrode active material contains a material containing carbon (C) as a constituent element, and the negative electrode binder contains at least one of polyvinylidene fluoride, polyimide, and aromatic polyamide.
[0003] Prior Art Documents
[0004] Patent Documents
[0005] Patent Document 1: International Publication No. 2018 / 146865 Summary of the Invention
[0006] Problems to be Solved by the Invention
[0007] An object of the present invention is to provide a negative electrode mixture capable of forming a negative electrode material layer having excellent flexibility and extremely firmly adhering to a metal foil, and capable of obtaining a battery having excellent cycle characteristics and a low gas increase rate after repeated charge and discharge.
[0008] Means for Solving the Problems
[0009] According to the present invention, there is provided a negative electrode mixture containing single-walled carbon nanotubes, a negative electrode active material, and a binder. As the negative electrode active material, a negative electrode active material having a potential of 2.5 V or less based on Li when alloying with Li or binding to Li is contained. The binder contains a fluorine-containing copolymer, and the fluorine-containing copolymer contains a vinylidene fluoride unit and other monomer units other than vinylidene fluoride.
[0010] The negative electrode active material is preferably a compound containing at least one element selected from the group consisting of Si, Sn, V, Nb, and Ti.
[0011] The negative electrode active material is preferably at least one selected from the group consisting of Si and SiO x (0 < x < 2).
[0012] The negative electrode active material is preferably a carbonaceous material.
[0013] The negative electrode active material is preferably a compound containing at least one element selected from the group consisting of Si, Sn, V, Nb and Ti, and a carbonaceous material.
[0014] The average outer diameter of the single-walled carbon nanotubes is preferably 2.5 nm or less.
[0015] The average G / D ratio of the single-walled carbon nanotubes is preferably 2 or more.
[0016] The content of the single-walled carbon nanotubes is preferably 0.001% by mass to 10% by mass based on the solid content mass of the negative electrode mixture.
[0017] The other monomers are preferably fluorinated monomers (but not including vinylidene fluoride units).
[0018] The other monomer is preferably at least one selected from the group consisting of tetrafluoroethylene, chlorotrifluoroethylene, (meth)acrylic acid, 2,3,3,3-tetrafluoropropylene, hexafluoropropylene, and fluoroalkyl vinyl ether.
[0019] The above-mentioned binder preferably further contains polyvinylidene fluoride.
[0020] The mass ratio of the polyvinylidene fluoride to the fluorine-containing copolymer (polyvinylidene fluoride / fluorine-containing copolymer) is preferably 99 / 1 to 1 / 99.
[0021] The negative electrode mixture of the present invention preferably further contains a solvent.
[0022] According to the present invention, there is provided a negative electrode comprising a current collector and a negative electrode material layer, wherein the negative electrode material layer is provided on one surface or both surfaces of the current collector and is formed of the negative electrode mixture.
[0023] Furthermore, according to the present invention, there is provided a secondary battery including the above-mentioned negative electrode.
[0024] Effects of the Invention
[0025] According to the present invention, a negative electrode mixture can be provided which can form a negative electrode material layer having excellent flexibility and extremely firmly adhering to a metal foil, and can obtain a battery having excellent cycle characteristics and a low gas increase rate after repeated charge and discharge. DETAILED DESCRIPTION
[0026] Hereinafter, specific embodiments of the present invention will be described in detail, but the present invention is not limited to the following embodiments.
[0027] The negative electrode mixture of the present invention contains single-walled carbon nanotubes, a negative electrode active material and a binder.
[0028] Patent Document 1 proposes suppressing expansion and contraction of a negative electrode during charge and discharge by forming a negative electrode active material layer including a first negative electrode active material containing a silicon-based material and a second negative electrode active material containing a carbon-based material.
[0029] The inventor has studied the means of suppressing the battery performance degradation caused by the expansion and contraction of the negative electrode during the charge and discharge of the negative electrode from a completely different point of view from the past. And it is found that by using a single-layer carbon nanotube and a fluorinated copolymer containing other monomer units other than vinylidene fluoride units and vinylidene fluoride as a binder, it is not only possible to form a negative electrode material layer that is extremely firmly fitted to the metal foil, but also the flexibility of the obtained negative electrode material layer is improved, even in the case of expansion and contraction of the negative electrode during charge and discharge, it is possible to obtain a battery with excellent cycle characteristics and low gas increase rate after repeated charge and discharge. The reason is not clear, but it is speculated that it is because the single-layer carbon nanotube forms a three-dimensional network structure in the negative electrode material layer that is difficult to be cut off even due to the volume change of the negative electrode, and by containing a binder containing a fluorinated copolymer, the flexibility is excellent, and the three-dimensional network structure is maintained for a long time in the negative electrode material layer that is firmly fitted to the metal foil (collector).
[0030] (Single-walled carbon nanotube)
[0031] Single-walled carbon nanotubes (SWCNTs) are a special type of carbon material known as a one-dimensional material. Single-walled carbon nanotubes are composed of sheets of graphene, rolled up to form a hollow tube with a wall of 1 atom thickness. By having this chemical structure and size, single-walled carbon nanotubes show excellent mechanical, electrical, thermal and optical properties.
[0032] The average outer diameter of the single-walled carbon nanotube is preferably 2.5 nm or less, more preferably 2.0 nm or less, and further preferably 1.8 nm or less, and preferably 1.0 nm or more, more preferably 1.1 nm or more, and further preferably 1.2 nm or more. The average outer diameter of the single-walled carbon nanotube can be obtained from the light absorption spectrum of the single-walled carbon nanotube obtained by ultraviolet visible near infrared spectroscopy (UV-Vis-NIR), Raman spectrum, or transmission electron microscope (TEM) image.
[0033] The average G / D ratio of the single-walled carbon nanotube measured by Raman spectroscopy (wavelength 532nm) is preferably 2 or more, more preferably 5 or more, further preferably 10 or more, particularly preferably 30 or more, most preferably 40 or more, preferably 250 or less, more preferably 220 or less, and further preferably 180 or less. The G / D ratio refers to the intensity ratio (G / D) of the G band and the D band of the Raman spectrum of the single-walled carbon nanotube. The higher the G / D ratio of the single-walled carbon nanotube, the higher the crystallinity of the single-walled carbon nanotube, and the fewer carbon nanotubes with impurity carbon and defects.
[0034] The average length of the single-walled carbon nanotubes is preferably from 0.1 μm to 50 μm, more preferably from 0.5 μm to 20 μm, and still more preferably from 1 μm to 10 μm. The average length of the single-walled carbon nanotubes can be determined as follows: Using an atomic force microscope (AFM), an AFM image of the single-walled carbon nanotubes is obtained, or using a transmission electron microscope (TEM), a TEM image of the single-walled carbon nanotubes is obtained, the length of each single-walled carbon nanotube is measured, and the sum of the lengths is divided by the number of single-walled carbon nanotubes measured, whereby the average length is obtained.
[0035] The content of the single-walled carbon nanotubes in the negative electrode binder is preferably from 0.001% by mass to 10% by mass, more preferably from 0.01% by mass to 2% by mass, and still more preferably from 0.01% by mass to 1% by mass, relative to the mass of the solid components of the negative electrode binder. When the content of the single-walled carbon nanotubes is within the above range, a three-dimensional network structure of the single-walled carbon nanotubes can be sufficiently formed in the obtained negative electrode material layer.
[0036] (Negative electrode active material)
[0037] The negative electrode binder of the present invention contains a negative electrode active material (excluding single-walled carbon nanotubes) that exhibits a potential of 2.5 V or less based on Li when alloying with Li or binding to Li as the negative electrode active material.
[0038] As the negative electrode active material, a negative electrode active material containing a metal can be used. The metal contained in the negative electrode active material is usually a metal that can electrochemically alloy with alkali metals such as Li and Na.
[0039] As the negative electrode active material, examples include metal elements such as Si, Zn, Sn, W, Al, Sb, Ge, Bi, and In that can electrochemically alloy with Li; alloys containing Si, Zn, Sn, W, Al, Sb, Ge, Bi, and In; lithium alloys such as lithium aluminum alloy and lithium tin alloy; metal oxides such as tin oxide and silicon oxide; and lithium titanate. As the negative electrode active material, one or more of them can be used.
[0040] As the negative electrode active material, a compound containing at least one element selected from the group consisting of Si, Sn, V, Nb, and Ti is preferably used, more preferably Si (Si element), an oxide of Si, an alloy containing Si, Sn (Sn carrier), an oxide of Sn, and an alloy containing Sn, and still more preferably at least one selected from the group consisting of Si and SiO x (0 < x < 2).
[0041] In addition, as the negative electrode active material, a carbonaceous material such as graphite powder can also be used. The carbonaceous material can be used together with the negative electrode active material containing a metal. Examples of the carbonaceous material include natural graphite, artificial carbonaceous materials, artificial graphite materials, thermal decomposition products of organic substances such as carbonaceous materials {such as natural graphite, coal-based coke, petroleum-based coke, coal-based asphalt, petroleum-based asphalt, or substances obtained by oxidation treatment of these asphalts, needle coke, pitch coke and carbon materials obtained by partially graphitizing them, furnace black, acetylene black, Ketjen black, asphalt-based carbon fibers, etc., organic substances that can be carbonized (such as coal tar pitch from soft asphalt to hard asphalt, or coal-based heavy oils such as dry distillation liquefied oil, straight-run heavy oils such as atmospheric residual oil and vacuum residual oil, decomposed petroleum heavy oils such as ethylene tar produced as a by-product during thermal decomposition of crude oil, naphtha, etc., and aromatic hydrocarbons such as acenaphthylene, decacyclic ene, anthracene, phenanthrene, N-ring compounds such as phenazine or acridine, thiophene, bithiophene, etc. S-ring compounds, biphenyl, terphenyl and other polyphenyls, polyvinyl chloride, polyvinyl alcohol, polyvinyl butyral, insolubilized products of these substances, nitrogen-containing organic polymers such as polyacrylonitrile and polypyrrole, sulfur-containing organic polymers such as polythiophene and polystyrene, natural polymers such as polysaccharides represented by cellulose, lignin, mannan, polygalacturonic acid, chitosan, and sucrose, thermoplastic resins such as polyphenylene sulfide and polyphenylene ether, thermosetting resins such as furfuryl alcohol resin, phenol-formaldehyde resin, and imide resin) and their carbides, or solutions obtained by dissolving carbonizable organic matter in low molecular weight organic solvents such as benzene, toluene, xylene, quinoline, and n-hexane, and their carbides} carbonaceous materials obtained by heat treatment at a temperature in the range of 400°C to 3200°C one or more.
[0042] When the negative electrode mixture contains a metal-containing negative electrode active material and a carbonaceous material, the mass ratio of the metal-containing negative electrode active material to the carbonaceous material is preferably 1 / 99 to 99 / 1, more preferably 5 / 95 to 95 / 5, and further preferably 10 / 90 to 90 / 10.
[0043] The content of the negative electrode active material in the negative electrode mixture is preferably 80.0% by mass to 99.9% by mass, and more preferably 90.0% by mass to 99.0% by mass, based on the mass of the negative electrode mixture.
[0044] (Binder)
[0045] The binder contained in the negative electrode mixture of the present invention contains a fluorinated copolymer containing vinylidene fluoride (VdF) units and other monomer units other than VdF. The other monomers may be fluorinated monomers or non-fluorinated monomers.
[0046] Examples of the fluorinated monomer (excluding VdF) include tetrafluoroethylene (TFE), vinyl fluoride, trifluoroethylene, chlorotrifluoroethylene (CTFE), fluoroalkyl vinyl ether, hexafluoropropylene (HFP), (perfluoroalkyl)ethylene, 2,3,3,3-tetrafluoropropylene, and trans-1,3,3,3-tetrafluoropropylene.
[0047] The fluoroalkyl vinyl ether is preferably a fluoroalkyl vinyl ether having a fluoroalkyl group having 1 to 5 carbon atoms, and more preferably at least one selected from the group consisting of perfluoro(methyl vinyl ether) (PMVE), perfluoro(ethyl vinyl ether) and perfluoro(propyl vinyl ether).
[0048] The fluorinated monomer is preferably at least one selected from the group consisting of TFE, CTFE, 2,3,3,3-tetrafluoropropylene, HFP and fluoroalkyl vinyl ether, more preferably at least one selected from the group consisting of TFE and HFP, and particularly preferably TFE.
[0049] The fluorinated monomer (excluding VdF) may or may not have a polar group.
[0050] Examples of the non-fluorinated monomer include non-fluorinated monomers having no polar group such as ethylene and propylene, and non-fluorinated monomers having a polar group (hereinafter sometimes referred to as a polar group-containing monomer).
[0051] If a substance having a polar group is used as a non-fluorinated monomer, the polar group is introduced into the copolymer, thereby obtaining a better adhesion between the coating layer and the metal foil. As the polar group, it is preferred to select at least one of the group consisting of a carbonyl-containing group, an epoxy group, a hydroxyl group, a sulfonic acid group, a sulfuric acid group, a phosphoric acid group, an amino group, an amide group and an alkoxy group, more preferably at least one of the group consisting of a carbonyl-containing group, an epoxy group and a hydroxyl group, and further preferably a carbonyl-containing group. The above-mentioned hydroxyl group does not include a hydroxyl group that constitutes a part of the above-mentioned carbonyl-containing group. In addition, the above-mentioned amino group is a monovalent functional group after removing hydrogen from ammonia, a primary amine or a secondary amine.
[0052] The above-mentioned carbonyl-containing group refers to a functional group having a carbonyl group (-C(=O)-). As the above-mentioned carbonyl-containing group, a group represented by the general formula: -COOR (R represents a hydrogen atom, an alkyl group or a hydroxyalkyl group) or a carboxylic anhydride group is preferred, and a group represented by the general formula: -COOR is more preferred. The number of carbon atoms of the alkyl group and the hydroxyalkyl group is preferably 1 to 16, more preferably 1 to 6, and further preferably 1 to 3. As the group represented by the general formula: -COOR, specifically, -COOCH2CH2OH, -COOCH2CH(CH3)OH, -COOCH(CH3)CH2OH, -COOH, -COOCH3, -COOC2H5, etc. can be mentioned. When the group represented by the general formula: -COOR is -COOH or contains -COOH, -COOH can be a carboxylate such as a metal carboxylate or an ammonium carboxylate.
[0053] In addition, the carbonyl-containing group may be a group represented by the general formula: -X-COOR (X is an atomic group with a molecular weight of 500 or less and a main chain consisting of 1 to 20 atoms, and R represents a hydrogen atom, an alkyl group or a hydroxyalkyl group). The number of carbon atoms in the alkyl group and the hydroxyalkyl group is preferably 1 to 16, more preferably 1 to 6, and even more preferably 1 to 3.
[0054] As the above-mentioned amide group, preferably, a group represented by the general formula: -CO-NRR' (R and R' independently represent a hydrogen atom or a substituted or unsubstituted alkyl group), or a bond represented by the general formula: -CO-NR"- (R" represents a hydrogen atom, a substituted or unsubstituted alkyl group or a substituted or unsubstituted phenyl group.).
[0055] Examples of the above-mentioned polar group-containing monomers include (meth) acrylate hydroxyalkyl esters such as hydroxyethyl acrylate and 2-hydroxypropyl acrylate; alkylidene malonates such as dimethyl methylene malonate; vinyl carboxyalkyl ethers such as vinyl carboxymethyl ether and vinyl carboxyethyl ether; (meth) acrylate carboxyalkyl esters such as 2-carboxyethyl acrylate and 2-carboxyethyl methacrylate; (meth) acryloyloxy ethyl succinate, acryloyloxypropyl succinate, methacryloyloxyethyl succinate, acryloyloxyethyl phthalate, methacryloyloxyethyl phthalate and other (meth) acryloyloxyalkyl dicarboxylates; monoesters of unsaturated dibasic acids such as monomethyl maleate, monoethyl maleate, monomethyl citraconic acid and monoethyl citraconic acid; general formula (4):
[0056] [Chemistry 1]
[0057]
[0058] (Where R 11 ~R 13 R independently represents a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms. 14represents a single bond or a hydrocarbon group having 1 to 8 carbon atoms. 1 represents an inorganic cation and / or an organic cation. ) represented by the monomer (4); unsaturated dibasic acids such as maleic acid, maleic anhydride, citraconic acid, citraconic anhydride, etc.; etc.
[0059] As the polar group-containing monomer unit which may be contained in the fluorinated copolymer, a unit based on a monomer (4) represented by the general formula (4) is preferred.
[0060] In the general formula (4), Y 1 represents an inorganic cation and / or an organic cation. Examples of inorganic cations include cations such as H, Li, Na, K, Mg, Ca, Al, and Fe. Examples of organic cations include NH4, NH3R 15 NH2R 15 2. NHR 15 3. NR 15 4(R 15 Each of the following independently represents an alkyl group having 1 to 4 carbon atoms. 1 , preferably H, Li, Na, K, Mg, Ca, Al, NH4, more preferably H, Li, Na, K, Mg, Al, NH4, further preferably H, Li, Al, NH4, and particularly preferably H. It should be noted that, for convenience, specific examples of inorganic cations and organic cations are recorded with symbols and valences omitted.
[0061] In the general formula (4), R 11 ~R 13 R independently represents a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms. The hydrocarbon group is a monovalent hydrocarbon group. The number of carbon atoms of the hydrocarbon group is preferably 4 or less. Examples of the hydrocarbon group include alkyl, alkenyl, alkynyl, etc. having the above-mentioned carbon number, preferably methyl or ethyl. 11 and R 12 R 13 Preferred is a hydrogen atom or a methyl group.
[0062] In the general formula (4), R 14 represents a single bond or a hydrocarbon group having 1 to 8 carbon atoms. The above hydrocarbon group is a divalent hydrocarbon group. The number of carbon atoms of the above hydrocarbon group is preferably 4 or less. Examples of the above hydrocarbon group include alkylene groups and alkenylene groups having the above carbon atoms, among which at least one selected from the group consisting of methylene, ethylene, ethylidene, propylidene and isopropylidene is preferred, and methylene is more preferred.
[0063] The monomer (4) is preferably at least one selected from the group consisting of (meth)acrylic acid and salts thereof, vinylacetic acid (3-butenoic acid) and salts thereof, 3-pentenoic acid and salts thereof, 4-pentenoic acid and salts thereof, 3-hexenoic acid and salts thereof, 4-heptenoic acid and salts thereof, and 5-hexenoic acid and salts thereof.
[0064] As the other monomer, at least one selected from the group consisting of TFE, CTFE, (meth)acrylic acid, 2,3,3,3-tetrafluoropropylene, HFP and fluoroalkyl vinyl ether is preferred. (Meth)acrylic acid includes acrylic acid and methacrylic acid.
[0065] The content of other monomer units in the fluorinated copolymer is preferably 0.0001 to 50.0 mol %, more preferably 0.01 mol % or more, further preferably 0.10 mol % or more, more preferably 45.0 mol % or less, further preferably 40.0 mol % or less, particularly preferably 35.0 mol % or less, based on all monomer units.
[0066] The content of the VdF unit in the fluorinated copolymer is 50.0 to 99.9999 mol %, more preferably 55.0 mol % or more, further preferably 60.0 mol % or more, particularly preferably 65.0 mol % or more, more preferably 99.99 mol % or less, further preferably 99.90 mol % or less, based on all monomer units.
[0067] When the fluorinated copolymer contains a fluorinated monomer unit as another monomer unit, the content of the fluorinated monomer unit is preferably 0.0001 mol% to 50.0 mol%, more preferably 2.0 mol% or more, further preferably 3.0 mol% or more, particularly preferably 4.0 mol% or more, more preferably 45.0 mol% or less, further preferably 40.0 mol% or less, particularly preferably 35.0 mol% or less, based on the total monomer units.
[0068] When the fluorinated copolymer contains a fluorinated monomer unit as another monomer unit, the content of the VdF unit of the fluorinated copolymer is 50.0 mol% to 99.999 mol% relative to all the monomer units, more preferably 55.0 mol% or more, further preferably 60.0 mol% or more, particularly preferably 65.0 mol% or more, more preferably 98.0 mol% or less, further preferably 97.0 mol% or less, particularly preferably 96.0 mol% or less.
[0069] When the fluorinated copolymer contains non-fluorinated monomer units such as polar group-containing monomers as other monomer units, the content of the non-fluorinated monomer units is preferably 0.0001 mol% to 50.0 mol%, more preferably 0.01 mol% or more, further preferably 0.10 mol% or more, more preferably 5.0 mol% or less, further preferably 3.0 mol% or less, particularly preferably 1.5 mol% or less, based on the total monomer units.
[0070] When the fluorinated copolymer contains a non-fluorinated monomer unit as another monomer unit, the content of the VdF unit of the fluorinated copolymer is preferably 50.0 mol% to 99.999 mol% based on all the monomer units, more preferably 95.0 mol% or more, further preferably 97.0 mol% or more, particularly preferably 98.5 mol% or more, more preferably 99.99 mol% or less, further preferably 99.90 mol% or less.
[0071] In the present invention, the composition of the fluorinated copolymer can be, for example, 19 When the fluorinated copolymer contains a polar group-containing monomer unit as another monomer unit, the content of the polar group-containing monomer unit can be measured by acid-base titration of the acid group, for example, when the polar group is an acid group such as carboxylic acid.
[0072] The weight average molecular weight (in terms of polystyrene) of the fluorinated copolymer is preferably 10,000 to 3,000,000, more preferably 30,000 or more, further preferably 50,000 or more, particularly preferably 200,000 or more, more preferably 2,400,000 or less, further preferably 2,200,000 or less, particularly preferably 2,000,000 or less. The weight average molecular weight can be measured by gel permeation chromatography (GPC) using dimethylformamide as a solvent.
[0073] The number average molecular weight (in terms of polystyrene) of the fluorinated copolymer is preferably 7,000 to 1,500,000, more preferably 21,000 or more, further preferably 35,000 or more, more preferably 1,400,000 or less, further preferably 1,200,000 or less, particularly preferably 1,100,000 or less. The number average molecular weight can be measured by gel permeation chromatography (GPC) using dimethylformamide as a solvent.
[0074] Examples of the fluorinated copolymer include VdF / (meth)acrylic acid copolymers, VdF / TFE copolymers, VdF / HFP copolymers, VdF / fluoroalkyl vinyl ether copolymers, VdF / TFE / HFP copolymers, VdF / 2,3,3,3-tetrafluoropropylene copolymers, VdF / TFE / 2,3,3,3-tetrafluoropropylene copolymers, VdF / TFE / (meth)acrylic acid copolymers, VdF / HFP / (meth)acrylic acid copolymers, VdF / CTFE copolymers, VdF / TFE / 4 -pentenoic acid copolymer, VdF / TFE / 3-butenoic acid copolymer, VdF / TFE / HFP / (meth)acrylic acid copolymer, VdF / TFE / HFP / 4-pentenoic acid copolymer, VdF / TFE / HFP / 3-butenoic acid copolymer, VdF / TFE / 2-carboxyethyl acrylate copolymer, VdF / TFE / HFP / 2-carboxyethyl acrylate copolymer, VdF / TFE / succinic acid acryloyloxyethyl ester copolymer, VdF / TFE / HFP / succinic acid acryloyloxyethyl ester copolymer, etc.
[0075] Among them, the fluorinated copolymer is preferably at least one selected from the group consisting of VdF / TFE copolymers, VdF / CTFE copolymers, VdF / (meth)acrylic acid copolymers, VdF / 2,3,3,3-tetrafluoropropylene copolymers, VdF / HFP copolymers and VdF / fluoroalkyl vinyl ether copolymers.
[0076] The VdF / TFE copolymer contains a VdF unit and a TFE unit. By using the VdF / TFE copolymer as a copolymer, a negative electrode mixture can be formed very easily, and a negative electrode mixture with excellent slurry stability can be obtained, and a coating layer with excellent softness can be formed. As the content of the VdF unit, relative to all monomer units of the VdF / TFE copolymer, it is preferably 50.0 mol% to 95.0 mol%, more preferably 55.0 mol% or more, further preferably 60.0 mol% or more, more preferably 92.0 mol% or less, and further preferably 89.0 mol% or less. As the content of the TFE unit, relative to all monomer units of the VdF / TFE copolymer, it is preferably 50.0 mol% to 5.0 mol%, more preferably 45.0 mol% or less, further preferably 40.0 mol% or less, more preferably 8.0 mol% or more, and further preferably 11.0 mol% or more.
[0077] In addition to the VdF unit and the TFE unit, the VdF / TFE copolymer may also include units based on monomers copolymerizable with VdF and TFE (wherein, excluding VdF and TFE). From the aspect of resistance to electrolyte swelling, the content of the units based on monomers copolymerizable with VdF and TFE is preferably less than 3.0 mol% relative to all monomer units of the VdF / TFE copolymer.
[0078] Examples of the monomer copolymerizable with VdF and TFE include the above-mentioned fluorinated monomers, the above-mentioned non-fluorinated monomers, etc. The monomer copolymerizable with VdF and TFE is preferably at least one selected from the group consisting of fluorinated monomers and polar group-containing monomers, and more preferably at least one selected from the group consisting of HFP, 2,3,3,3-tetrafluoropropylene and monomer (4).
[0079] The weight average molecular weight (polystyrene equivalent) of the VdF / TFE copolymer is preferably 50,000 to 2,000,000, more preferably 80,000 to 1,700,000, and even more preferably 100,000 to 1,500,000.
[0080] The number average molecular weight (polystyrene equivalent) of the VdF / TFE copolymer is 35,000 to 1,400,000, more preferably 40,000 to 1,300,000, and even more preferably 50,000 to 1,200,000.
[0081] The VdF / CTFE copolymer contains VdF units and CTFE units. By using the VdF / CTFE copolymer as a copolymer, a negative electrode mixture can be formed very easily, and a coating layer that is extremely firmly bonded to the metal foil can be formed. As the content of the VdF unit, relative to all monomer units of the VdF / CTFE copolymer, it is preferably 80.0 mol% to 98.0 mol%, more preferably 85.0 mol% or more, further preferably 90.0 mol% or more, more preferably 97.5 mol% or less, and further preferably 97.0 mol% or less. As the content of the CTFE unit, relative to all monomer units of the VdF / CTFE copolymer, it is preferably 20.0 mol% to 2.0 mol%, more preferably 15.0 mol% or less, further preferably 10.0 mol% or less, more preferably 2.5 mol% or more, and further preferably 3.0 mol% or more.
[0082] In addition to VdF units and CTFE units, the VdF / CTFE copolymer may also include units based on monomers copolymerizable with VdF and CTFE (wherein, VdF and CTFE are not included). From the aspect of resistance to electrolyte swelling, the content of units based on monomers copolymerizable with VdF and CTFE is preferably 3.0 mol% or less relative to all monomer units of the VdF / CTFE copolymer.
[0083] Examples of the monomer copolymerizable with VdF and CTFE include the above-mentioned fluorinated monomers, the above-mentioned non-fluorinated monomers, etc. The monomer copolymerizable with VdF and CTFE is preferably at least one selected from the group consisting of fluorinated monomers and polar group-containing monomers, more preferably at least one selected from the group consisting of TFE, HFP, 2,3,3,3-tetrafluoropropylene and monomer (4), and even more preferably TFE.
[0084] The weight average molecular weight (polystyrene equivalent) of the VdF / CTFE copolymer is preferably 50,000 to 2,000,000, more preferably 80,000 to 1,700,000, and even more preferably 100,000 to 1,500,000.
[0085] The number average molecular weight (polystyrene equivalent) of the VdF / CTFE copolymer is preferably 35,000 to 1,400,000, more preferably 40,000 to 1,300,000, and even more preferably 50,000 to 1,200,000.
[0086] The VdF / (meth)acrylic acid copolymer contains a VdF unit and a (meth)acrylic acid unit. By using the VdF / (meth)acrylic acid copolymer as a copolymer, a negative electrode mixture can be formed very easily, and a coating layer that is extremely firmly bonded to the metal foil can be formed. The content of the (meth)acrylic acid unit is preferably 0.0001 mol% to 5.0 mol%, more preferably 0.01 mol% to 3.0 mol%, and further preferably 0.10 mol% to 1.5 mol% relative to the total monomer units.
[0087] The content of the VdF unit in the VdF / (meth)acrylic acid copolymer is preferably 95.0 to 99.9999 mol %, more preferably 97.0 to 99.99 mol %, and even more preferably 98.5 to 99.90 mol %, based on all monomer units.
[0088] The weight average molecular weight (polystyrene equivalent) of the VdF / (meth)acrylic acid copolymer is preferably 50,000 to 3,000,000, more preferably 80,000 or more, further preferably 100,000 or more, particularly preferably 200,000 or more, more preferably 2,400,000 or less, further preferably 2,200,000 or less, particularly preferably 2,000,000 or less.
[0089] The number average molecular weight (polystyrene equivalent) of the VdF / (meth)acrylic acid copolymer is preferably 20,000 to 1,500,000, more preferably 40,000 or more, further preferably 70,000 or more, particularly preferably 140,000 or more, more preferably 1,400,000 or less, further preferably 1,200,000 or less, particularly preferably 1,100,000 or less.
[0090] The VdF / 2,3,3,3-tetrafluoropropylene copolymer contains a VdF unit and a 2,3,3,3-tetrafluoropropylene unit. By using the VdF / 2,3,3,3-tetrafluoropropylene copolymer as a copolymer, a negative electrode mixture can be formed very easily, and a coating layer with excellent flexibility and conductivity can be formed. The content of the VdF unit is preferably 50.0 mol% to 98.0 mol% relative to all monomer units of the VdF / 2,3,3,3-tetrafluoropropylene copolymer, more preferably 55.0 mol% or more, further preferably 60.0 mol% or more, particularly preferably 65.0 mol% or more, more preferably 97.0 mol% or less, and further preferably 96.0 mol% or less. The content of the 2,3,3,3-tetrafluoropropylene units is preferably 2.0 mol% to 50.0 mol% relative to all monomer units of the VdF / TFE copolymer, more preferably 3.0 mol% or more, further preferably 4.0 mol% or more, more preferably 45.0 mol% or less, further preferably 40.0 mol% or less, particularly preferably 35.0 mol% or less.
[0091] In addition to the VdF unit and the 2,3,3,3-tetrafluoropropylene unit, the VdF / 2,3,3,3-tetrafluoropropylene copolymer may further include a unit based on a monomer copolymerizable with VdF and 2,3,3,3-tetrafluoropropylene (wherein VdF and 2,3,3,3-tetrafluoropropylene are not included). From the aspect of resistance to swelling of the electrolyte, the content of the unit based on a monomer copolymerizable with VdF and 2,3,3,3-tetrafluoropropylene is preferably 3.0 mol% or less relative to the total monomer units of the VdF / 2,3,3,3-tetrafluoropropylene copolymer.
[0092] Examples of the monomer copolymerizable with VdF and 2,3,3,3-tetrafluoropropylene include the above-mentioned fluorinated monomers, the above-mentioned non-fluorinated monomers, etc. The monomer copolymerizable with VdF and 2,3,3,3-tetrafluoropropylene is preferably at least one selected from the group consisting of fluorinated monomers and polar group-containing monomers, and more preferably at least one selected from the group consisting of TFE, HFP, and monomer (4).
[0093] The weight average molecular weight (polystyrene equivalent) of the VdF / 2,3,3,3-tetrafluoropropylene copolymer is preferably 10,000 to 2,000,000, more preferably 30,000 to 1,700,000, and even more preferably 5,000 to 1,500,000.
[0094] The number average molecular weight (polystyrene equivalent) of the VdF / 2,3,3,3-tetrafluoropropylene copolymer is preferably 7,000 to 1,400,000, more preferably 21,000 to 1,300,000, and even more preferably 35,000 to 1,200,000.
[0095] The VdF / HFP copolymer contains a VdF unit and an HFP unit. By using the VdF / HFP copolymer as a copolymer, a negative electrode mixture can be formed very easily, and a coating layer that is extremely firmly bonded to the metal foil can be formed. As the content of the VdF unit, relative to all monomer units of the VdF / HFP copolymer, it is preferably 80.0 mol% to 98.0 mol%, more preferably 83.0 mol% or more, further preferably 85.0 mol% or more, more preferably 97.0 mol% or less, and further preferably 96.0 mol% or less. As the content of the HFP unit, relative to all monomer units of the VdF / HFP copolymer, it is preferably 20.0 mol% to 2.0 mol%, more preferably 17.0 mol% or less, further preferably 15.0 mol% or less, more preferably 3.0 mol% or more, and further preferably 4.0 mol% or more.
[0096] In addition to the VdF unit and the HFP unit, the VdF / HFP copolymer may also include units based on monomers that can copolymerize with VdF and HFP (wherein, excluding VdF and HFP). From the aspect of resistance to electrolyte swelling, the content of the units based on monomers that can copolymerize with VdF and HFP is preferably less than 3.0 mol % relative to all monomer units of the VdF / HFP copolymer.
[0097] Examples of the monomer copolymerizable with VdF and HFP include the above-mentioned fluorinated monomers, the above-mentioned non-fluorinated monomers, etc. The monomer copolymerizable with VdF and HFP is preferably at least one selected from the group consisting of fluorinated monomers and polar group-containing monomers, more preferably at least one selected from the group consisting of TFE, 2,3,3,3-tetrafluoropropylene and monomer (4), and still more preferably monomer (4).
[0098] The weight average molecular weight (polystyrene equivalent) of the VdF / HFP copolymer is preferably 50,000 to 2,000,000, more preferably 80,000 to 1,700,000, and even more preferably 100,000 to 1,500,000.
[0099] The number average molecular weight (polystyrene equivalent) of the VdF / HFP copolymer is preferably 35,000 to 1,400,000, more preferably 40,000 to 1,300,000, and even more preferably 50,000 to 1,200,000.
[0100] The VdF / fluoroalkyl vinyl ether copolymer contains VdF units and fluoroalkyl vinyl ether units. As the content of the VdF unit, relative to the total monomer units of the VdF / fluoroalkyl vinyl ether copolymer, it is preferably 80.0 mol% to 98.0 mol%, more preferably 83.0 mol% or more, further preferably 85.0 mol% or more, more preferably 97.0 mol% or less, and further preferably 96.0 mol% or less. As the content of the fluoroalkyl vinyl ether unit, relative to the total monomer units of the VdF / fluoroalkyl vinyl ether copolymer, it is preferably 20.0 mol% to 2.0 mol%, more preferably 17.0 mol% or less, further preferably 15.0 mol% or less, more preferably 3.0 mol% or more, and further preferably 4.0 mol% or more.
[0101] In addition to the VdF unit and the fluoroalkyl vinyl ether unit, the VdF / fluoroalkyl vinyl ether copolymer may also include units based on monomers copolymerizable with VdF and fluoroalkyl vinyl ether (wherein, excluding VdF and fluoroalkyl vinyl ether). From the aspect of resistance to electrolyte swelling, the content of the units based on monomers copolymerizable with VdF and fluoroalkyl vinyl ether is preferably less than 3.0 mol% relative to all monomer units of the VdF / fluoroalkyl vinyl ether copolymer.
[0102] Examples of monomers copolymerizable with VdF and fluoroalkyl vinyl ether include the above-mentioned fluorinated monomers, the above-mentioned non-fluorinated monomers, etc. As monomers copolymerizable with VdF and fluoroalkyl vinyl ether, at least one selected from the group consisting of fluorinated monomers and polar group-containing monomers is preferred, at least one selected from the group consisting of TFE, 2,3,3,3-tetrafluoropropylene and monomer (4) is more preferred, and monomer (4) is further preferred.
[0103] The weight average molecular weight (polystyrene equivalent) of the VdF / fluoroalkyl vinyl ether copolymer is preferably 50,000 to 2,000,000, more preferably 80,000 to 1,700,000, and even more preferably 100,000 to 1,500,000.
[0104] The number average molecular weight (polystyrene equivalent) of the VdF / fluoroalkyl vinyl ether copolymer is preferably 35,000 to 1,400,000, more preferably 40,000 to 1,300,000, and even more preferably 50,000 to 1,200,000.
[0105] The binder also preferably contains polyvinylidene fluoride (PVdF). PVdF is a polymer containing VdF units, and is a polymer different from the above-mentioned fluorine-containing copolymer. PVdF may be a VdF homopolymer consisting only of VdF units, or a polymer containing VdF units and units based on a monomer copolymerizable with VdF.
[0106] In the above PVdF, the monomer copolymerizable with VdF is preferably a monomer different from tetrafluoroethylene (TFE). That is, PVdF preferably does not contain a TFE unit.
[0107] In the above-mentioned PVdF, as the monomer that can be copolymerized with VdF, fluorinated monomers, non-fluorinated monomers, etc. can be mentioned, preferably fluorinated monomers. As the above-mentioned fluorinated monomers, vinyl fluoride, trifluoroethylene, chlorotrifluoroethylene (CTFE), fluoroalkyl vinyl ether, hexafluoropropylene (HFP), (perfluoroalkyl) ethylene, 2,3,3,3-tetrafluoropropylene, trans-1,3,3,3-tetrafluoropropylene, etc. can be mentioned. As the above-mentioned non-fluorinated monomers, ethylene, propylene, etc. can be mentioned.
[0108] In the above PVdF, the monomer copolymerizable with VdF is preferably at least one fluorinated monomer selected from the group consisting of CTFE, fluoroalkyl vinyl ether, HFP and 2,3,3,3-tetrafluoropropylene, and more preferably at least one fluorinated monomer selected from the group consisting of CTFE, HFP and fluoroalkyl vinyl ether.
[0109] In the above PVdF, the content of the monomer units copolymerizable with VdF is preferably 0 to 5.0 mol%, more preferably 0 to 3.0 mol%, relative to all monomer units. In PVdF, the content of the fluorinated monomer units copolymerizable with VdF is preferably less than 5.0 mol%, more preferably less than 3.0 mol%, and further preferably less than 1.0 mol%, relative to all monomer units.
[0110] In the present invention, the composition of PVdF can be, for example, 19 The results were determined by F-NMR measurement.
[0111] The PVdF may have a polar group. As the polar group, there is no particular limitation as long as it is a polar functional group, preferably at least one selected from the group consisting of a carbonyl-containing group, an epoxy group, a hydroxyl group, a sulfonic acid group, a sulfuric acid group, a phosphoric acid group, an amino group, an amide group and an alkoxy group, more preferably at least one selected from the group consisting of a carbonyl-containing group, an epoxy group and a hydroxyl group, and further preferably a carbonyl-containing group. The hydroxyl group does not include a hydroxyl group that constitutes a part of the carbonyl-containing group. In addition, the amino group is a monovalent functional group after removing hydrogen from ammonia, a primary amine or a secondary amine.
[0112] The above-mentioned carbonyl-containing group refers to a functional group having a carbonyl group (-C(=O)-). As the above-mentioned carbonyl-containing group, a group represented by the general formula: -COOR (R represents a hydrogen atom, an alkyl group or a hydroxyalkyl group) or a carboxylic anhydride group is preferred, and a group represented by the general formula: -COOR is more preferred. The number of carbon atoms of the alkyl group and the hydroxyalkyl group is preferably 1 to 16, more preferably 1 to 6, and further preferably 1 to 3. As the group represented by the general formula: -COOR, specifically, -COOCH2CH2OH, -COOCH2CH(CH3)OH, -COOCH(CH3)CH2OH, -COOH, -COOCH3, -COOC2H5, etc. can be mentioned. When the group represented by the general formula: -COOR is -COOH or contains -COOH, -COOH can be a carboxylate such as a metal carboxylate or an ammonium carboxylate.
[0113] In addition, the carbonyl-containing group may be a group represented by the general formula: -X-COOR (the main chain of X is composed of 2 to 15 atoms, the molecular weight of the atomic group represented by X is preferably 350 or less, and R represents a hydrogen atom, an alkyl group or a hydroxyalkyl group). The number of carbon atoms in the alkyl group and the hydroxyalkyl group is preferably 1 to 16, more preferably 1 to 6, and even more preferably 1 to 3.
[0114] As the above-mentioned amide group, preferably, a group represented by the general formula: -CO-NRR' (R and R' independently represent a hydrogen atom or a substituted or unsubstituted alkyl group), or a bond represented by the general formula: -CO-NR"- (R" represents a hydrogen atom, a substituted or unsubstituted alkyl group or a substituted or unsubstituted phenyl group.).
[0115] The above-mentioned polar group can be introduced into PVdF by polymerizing VdF with a monomer having the above-mentioned polar group (hereinafter referred to as a monomer containing a polar group), or by reacting PVdF with a compound having the above-mentioned polar group. From the perspective of productivity, it is preferred to polymerize VdF with the above-mentioned monomer containing a polar group.
[0116] If VdF and the above-mentioned polar group-containing monomer are polymerized, PVdF containing VdF units and polar group-containing monomer units is obtained. That is, PVdF preferably contains the above-mentioned polar group-containing monomer units. The content of the above-mentioned polar group-containing monomer units relative to all monomer units is preferably 0.001 mol% to 5.0 mol%, more preferably 0.01 mol% to 3.0 mol%, and further preferably 0.10 mol% to 1.5 mol%.
[0117] In the present invention, for example, when the polar group is an acid group such as carboxylic acid, the content of the polar group-containing monomer unit in PVdF can be measured by acid-base titration of the acid group.
[0118] Examples of the above-mentioned polar group-containing monomers include hydroxyalkyl (meth)acrylates such as hydroxyethyl acrylate and 2-hydroxypropyl acrylate; unsaturated monobasic acids such as (meth)acrylic acid, crotonic acid, vinylacetic acid (3-butenoic acid), 3-pentenoic acid, 4-pentenoic acid, 3-hexenoic acid, and 4-heptenoic acid; unsaturated dibasic acids such as maleic acid, maleic anhydride, citraconic acid, and citraconic anhydride; alkylidene malonates such as dimethyl methylene malonate; vinyl carboxymethyl ether, vinyl carboxyethyl ether, and the like; Alkenyl carboxyl alkyl ether; (meth) carboxyl alkyl acrylates such as 2-carboxyethyl acrylate and 2-carboxyethyl methacrylate; (meth) acryloxyalkyl dicarboxylates such as acryloxyethyl succinate, methacryloyloxyethyl succinate, acryloxyethyl phthalate, acryloxypropyl succinate, and methacryloyloxyethyl phthalate; monoesters of unsaturated dibasic acids such as monomethyl maleate, monoethyl maleate, monomethyl citrate, and monoethyl citrate; etc.
[0119] When PVdF is reacted with a compound having the above-mentioned polar group and the above-mentioned polar group is introduced into PVdF, as the compound having the above-mentioned polar group, a silane coupling agent or a titanate coupling agent containing a monomer containing the above-mentioned polar group or PVdF and a reactive group and a hydrolyzable group can be used. As the above-mentioned hydrolyzable group, an alkoxy group is preferably used. When a coupling agent is used, the polar group can be added to PVdF by reacting with PVdF dissolved or swollen in a solvent.
[0120] As PVdF, it is also possible to use a material obtained by further reacting the partially dehydrofluorinated PVdF with an oxidant after the PVdF is partially dehydrofluorinated with an alkali. As the above-mentioned oxidant, hydrogen peroxide, hypochlorite, palladium halide, chromium halide, alkali metal permanganate, peroxide compound, alkyl peroxide, alkyl persulfate etc. can be enumerated.
[0121] The content of the VdF unit in PVdF is preferably more than 95.0 mol %, more preferably more than 97.0 mol %, and even more preferably more than 99.0 mol % based on all monomer units.
[0122] The content of the VdF unit in PVdF is preferably 95.0 mol% to 99.999 mol%, more preferably 97.0 mol% or more, further preferably 98.5 mol% or more, more preferably 99.99 mol% or less, further preferably 99.90 mol% or less, based on all monomer units.
[0123] The weight average molecular weight (polystyrene conversion) of PVdF is preferably 50,000 to 3,000,000, more preferably 80,000 or more, further preferably 100,000 or more, particularly preferably 200,000 or more, more preferably 2,400,000 or less, further preferably 2,200,000 or less, particularly preferably 2,000,000 or less. The weight average molecular weight can be measured by gel permeation chromatography (GPC) using N,N-dimethylformamide as a solvent. In addition, the weight average molecular weight of PVdF can be 1,000,000 or more, or 1,500,000 or more.
[0124] The number average molecular weight (polystyrene conversion) of PVdF is preferably 20,000 to 1,500,000, more preferably 40,000 or more, further preferably 70,000 or more, particularly preferably 140,000 or more, more preferably 1,400,000 or less, further preferably 1,200,000 or less, particularly preferably 1,100,000 or less. The number average molecular weight can be measured by gel permeation chromatography (GPC) using dimethylformamide as a solvent.
[0125] The melting point of PVdF is preferably 100° C. to 240° C. The melting point can be determined using a differential scanning calorimetry (DSC) apparatus as a temperature relative to a local maximum in a heat of fusion curve when the temperature is increased at a rate of 10° C. / min.
[0126] When the binder contains PVdF and a fluorinated copolymer, the mass ratio of PVdF to the fluorinated copolymer in the binder (PVdF / fluorinated copolymer) is preferably 99 / 1 to 1 / 99, more preferably 97 / 3 to 3 / 97, further preferably 95 / 5 to 5 / 95, further preferably 90 / 10 to 10 / 90, particularly preferably 85 / 15 to 15 / 85, and most preferably 80 / 20 to 40 / 60.
[0127] In addition to PVdF and the fluorine-containing copolymer, the binder may contain other polymers, such as polymethacrylate, polymethyl methacrylate, polyacrylonitrile, polyimide, polyamide, polyamideimide, polycarbonate, styrene rubber, butadiene rubber, etc.
[0128] The content of the fluorinated copolymer in the binder is preferably 1% by mass or more, more preferably 3% by mass or more, further preferably 5% by mass or more, particularly preferably 10% by mass or more, most preferably 15% by mass or more, based on the mass of the binder, and may be 100% by mass or less.
[0129] The content of the binder in the negative electrode mixture is preferably 0.1% by mass to 20% by mass, more preferably 0.2% by mass to 10% by mass, and even more preferably 0.5% by mass to 5% by mass, based on the mass of the negative electrode mixture.
[0130] (Solvent)
[0131] The negative electrode mixture of the present invention preferably contains a solvent. Examples of the solvent include water and an organic solvent. An organic solvent is preferred because it greatly reduces the possibility of water remaining in the negative electrode material layer when the negative electrode mixture is used to form the negative electrode material layer.
[0132] Examples of the organic solvent include nitrogen-containing organic solvents such as N-methyl-2-pyrrolidone, N,N-dimethylacetamide, and dimethylformamide; ketone solvents such as acetone, methyl ethyl ketone, cyclohexanone, and methyl isobutyl ketone; ester solvents such as ethyl acetate and butyl acetate; ether solvents such as tetrahydrofuran and dioxane; β-alkoxypropionamides such as β-methoxy-N,N-dimethylpropionamide, β-n-butoxy-N,N-dimethylpropionamide, and β-n-hexyloxy-N,N-dimethylpropionamide; and low-boiling-point general-purpose organic solvents such as mixed solvents thereof.
[0133] As the organic solvent, a solvent represented by the general formula (1) can also be used.
[0134] General formula (1):
[0135] [Chemistry 2]
[0136]
[0137] (Where R 1 , R 2 and R 3 are independently H or a monovalent substituent, wherein R 1 , R 2 and R 3 The total number of carbon atoms is 6 or more, R 1 , R 2 and R 3 At least one of R is an organic group having a carbonyl group. 1 , R 2 and R 3 Any two of them can be bonded to form a ring. )
[0138] As the solvent represented by the general formula (1), it is preferred that at least one selected from the group consisting of 3-methoxy-N,N-dimethylpropionamide, N-ethyl-2-pyrrolidone (NEP), N-butyl-2-pyrrolidone (NBP), acryloylmorpholine, N-cyclohexyl-2-pyrrolidone, N-vinyl-2-pyrrolidone, 3-butoxy-N,N-dimethylpropionamide, N,N,N',N'-tetraethyl urea, N,N-dimethylacetoacetamide, N-octyl-2-pyrrolidone and N,N-diethylacetamide.
[0139] As the solvent, water or at least one selected from the group consisting of N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone and a solvent represented by the general formula (1) is preferred from the viewpoint of excellent coating properties.
[0140] More preferably, at least one selected from the group consisting of N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, 3-methoxy-N,N-dimethylpropionamide, N-ethyl-2-pyrrolidone (NEP), N-butyl-2-pyrrolidone (NBP), acryloylmorpholine, N-cyclohexyl-2-pyrrolidone, N-vinyl-2-pyrrolidone, 3-butoxy-N,N-dimethylpropionamide, N,N,N',N'-tetraethylurea, N,N-dimethylacetoacetamide, N-octyl-2-pyrrolidone and N,N-diethylacetamide is used.
[0141] More preferably, at least one selected from the group consisting of N-methyl-2-pyrrolidone, N,N-dimethylacetamide, 3-methoxy-N,N-dimethylpropionamide, N-ethyl-2-pyrrolidone and N-butyl-2-pyrrolidone,
[0142] In particular, at least one selected from the group consisting of N-methyl-2-pyrrolidone and N,N-dimethylacetamide is preferred.
[0143] The amount of the solvent in the negative electrode mixture is determined in consideration of coating properties on the current collector, thin film forming properties after drying, etc. Usually, the ratio of the binder to the solvent is 0.5:99.5 to 20:80 in terms of mass ratio.
[0144] (Other ingredients)
[0145] The negative electrode mixture of the present invention may further contain other components such as a conductive auxiliary agent (excluding the carbonaceous material used as the negative electrode mixture), a leveling agent, and a reinforcing material.
[0146] The negative electrode mixture can be prepared, for example, by mixing single-layer carbon nanotubes, a binder and a solvent, and then adding a negative electrode active material to the obtained mixture and further mixing. Then, the obtained negative electrode mixture is evenly coated on a collector such as a metal foil or a metal mesh, dried, and pressed as needed to form a thin negative electrode material layer on the collector to prepare a thin film electrode. In addition, the negative electrode mixture can also be prepared by first mixing single-layer carbon nanotubes, a negative electrode active material and a binder and then adding a solvent.
[0147] (use)
[0148] The negative electrode mixture of the present invention can be suitably used as a material for forming a secondary battery. Even in the case of using a negative electrode active material that greatly expands in volume during charging and shrinks during discharge, by using the negative electrode mixture of the present invention, a negative electrode material layer with excellent flexibility and extremely firm adhesion to the metal foil can be formed, and a battery with excellent cycle characteristics and low gas increase rate after repeated charge and discharge can be obtained. Therefore, the negative electrode mixture of the present invention is suitable as a negative electrode mixture for the negative electrode of a secondary battery. The secondary battery to which the negative electrode mixture of the present invention is applied has a positive electrode formed by the positive electrode mixture being retained in the positive electrode collector, a negative electrode formed by the negative electrode mixture being retained in the negative electrode collector, and an electrolyte.
[0149] The negative electrode mixture of the present invention may be a negative electrode mixture for a secondary battery or a negative electrode mixture for a lithium ion secondary battery.
[0150] (negative electrode)
[0151] The negative electrode of the present invention comprises a current collector and a negative electrode material layer. The negative electrode material layer is formed using the negative electrode mixture of the present invention and can be provided on one side or both sides of the current collector.
[0152] Examples of the current collector included in the negative electrode of the present invention include metal foils and metal meshes made of iron, stainless steel, copper, aluminum, nickel, titanium, and the like. Among them, copper foil is preferred.
[0153] The negative electrode of the present invention can be suitably produced by a production method in which the negative electrode mixture of the present invention is applied to a current collector. After the negative electrode mixture is applied, the coating film can be further dried, optionally subjected to heat treatment, and the obtained dry coating film can be pressed.
[0154] (Secondary battery)
[0155] According to the present invention, there is provided a secondary battery comprising the above-mentioned negative electrode. The secondary battery of the present invention preferably comprises a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the negative electrode is the above-mentioned negative electrode.
[0156] The secondary battery of the present invention includes a negative electrode formed using the negative electrode mixture of the present invention, and therefore has a high cycle retention rate and a low gas increase rate.
[0157] The non-aqueous electrolyte is not particularly limited, and one or more of the known solvents such as propylene carbonate, ethylene carbonate, butylene carbonate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, etc. can be used. The electrolyte can also use a conventionally known electrolyte, and LiClO4, LiAsF6, LiPF6, LiBF4, LiCl, LiBr, CH3SO3Li, CF3SO3Li, cesium carbonate, etc. can be used.
[0158] The negative electrode of the present invention can be suitably used as a negative electrode for a wound-type secondary battery. In addition, the secondary battery of the present invention may be a wound-type secondary battery.
[0159] The electrode of the present invention can be used not only in the lithium ion secondary battery using a liquid electrolyte as described above as a non-aqueous electrolyte secondary battery, but also in a polymer electrolyte lithium secondary battery. In addition, it is also useful as an electric double layer capacitor.
[0160] Although the embodiments have been described above, it should be understood that various modifications may be made to the embodiments and details without departing from the spirit and scope of the claims.
[0161] Example
[0162] Next, embodiments of the present invention will be described with reference to examples, but the present invention is not limited to these examples.
[0163] Each numerical value in the examples was measured by the following method.
[0164] (Ratio of VdF unit to TFE unit in fluorinated copolymer)
[0165] The ratio of the VdF unit to the TFE unit in the fluorinated copolymer was determined using an NMR analyzer (VNS 400 MHz, manufactured by Agilent Technologies).19 F-NMR measurement was performed in a DMF-d7 solution state of the polymer.
[0166] pass 19 The following peak areas (A, B, C, and D) were determined by F-NMR measurement, and the ratio of the VdF unit to the TFE unit was calculated.
[0167] A: The area of the peak between -86ppm and -98ppm
[0168] B: The area of the peak between -105ppm and -118ppm
[0169] C: The area of the peak at -119 ppm to -122 ppm
[0170] D: The area of the peak between -122ppm and -126ppm
[0171] Ratio of VdF units: (4A+2B) / (4A+3B+2C+2D)×100 [mol %]
[0172] Ratio of TFE units: (B+2C+2D) / (4A+3B+2C+2D)×100 [mol %]
[0173] (Weight average molecular weight)
[0174] The measurement was performed by gel permeation chromatography (GPC). HLC-8320GPC and columns (three SuperAWM-H connected in series) manufactured by Tosoh Corporation were used, dimethylformamide (DMF) as a solvent was allowed to flow at a flow rate of 0.3 ml / min, and the weight average molecular weight was calculated from the measured data (reference: polystyrene).
[0175] (Melting Point)
[0176] Using a differential scanning calorimetry (DSC) apparatus, the temperature was raised from 30°C to 220°C at a rate of 10°C / min, then lowered to 30°C at 10°C / min, and then raised to 220°C at a rate of 10°C / min again, and the temperature corresponding to the maximum value in the heat of fusion curve at this time was determined as the melting point.
[0177] In the examples and comparative examples, a polymer having the following physical properties was used as a binder.
[0178] Binder (D): PVdF (VdF homopolymer)
[0179] Weight average molecular weight 1800000
[0180] Melting point 171℃
[0181] Binder (E): Fluorinated copolymer containing VdF units and TFE units
[0182] VdF / TFE=81 / 19 (mol%)
[0183] Weight average molecular weight 1230000
[0184] Melting point 128℃
[0185] CMC: Carboxymethyl cellulose
[0186] SBR: Styrene Butadiene Rubber
[0187] In addition, in Examples and Comparative Examples, the following negative electrode active materials were used.
[0188] SiO: Graphite-coated silicon oxide powder (a powder in which the surface of silicon oxide is coated with graphite)
[0189] Si: Silicon powder
[0190] Sn: Tin powder
[0191] LTO: Lithium Titanate
[0192] In addition, in Examples and Comparative Examples, the following conductive additives were used.
[0193] AB: Acetylene Black
[0194] Super P: Furnace black (trade name: Super-P (manufactured by Imerys)
[0195] KB: Ketchen Black
[0196] In addition, in the examples and comparative examples, the following single-walled carbon nanotubes were used.
[0197] Single-walled carbon nanotube (trade name: "TUBALL BATT SWCNT", manufactured by OCSiAl)
[0198] Average outer diameter: 1.6±0.4nm
[0199] Length: 5μm or more
[0200] Average G / D ratio: 86.5±7.1
[0201] (Preparation of negative electrode mixture)
[0202] Example 1
[0203] 93% by mass of the negative electrode active material, 0.05% by mass of the single-walled carbon nanotubes, 1.95% by mass of the conductive aid and 5% by mass of the binder were mixed, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was further added to prepare a negative electrode mixture having the composition shown in Tables 1 and 2. In the preparation of the negative electrode mixture, an NMP dispersion of the single-walled carbon nanotubes, an 8% by mass NMP solution of the binder (D), and a 5% by mass NMP solution of the binder (E) were used.
[0204] Examples 2 to 20, Comparative Examples 2 to 5
[0205] A negative electrode mixture was prepared in the same manner as in Example 1 except that the materials and the amounts used were changed so as to have the compositions shown in Tables 1 and 2. The amounts of the single-walled carbon nanotubes and the conductive additive were adjusted so that the total content was 2% by mass.
[0206] Comparative Example 3
[0207] 93 mass % of negative electrode active material, 0.5 mass % of single-walled carbon nanotubes, 1.55 mass % of conductive aid and 5 mass % of binder were mixed, and then an appropriate amount of water was added to prepare a negative electrode mixture having a composition shown in Table 2. In the preparation of the negative electrode mixture, an aqueous dispersion of single-walled carbon nanotubes, a 48 mass % aqueous solution of SBR, and a 1.5 mass % aqueous solution of CMC were used.
[0208] (Fabrication of Negative Electrode Having Negative Electrode Material Layer)
[0209] The negative electrode mixture obtained in the embodiment and the comparative example is applied to one or both sides of the negative electrode collector formed by copper foil, and dried. It is cut into a predetermined electrode size and rolled using a roller press to prepare a negative electrode having a negative electrode material layer formed on one or both sides of the negative electrode collector, and evaluated by the following method.
[0210] (Peel strength between negative electrode material layer and negative electrode current collector)
[0211] Cut the negative electrode with a negative electrode material layer on one side to make a 1.2 cm × 7.0 cm test piece. After fixing the negative electrode material layer side of the test piece to a movable fixture with double-sided tape, stick the tape on the surface of the negative electrode collector and stretch the tape along 90 degrees at a speed of 100 mm / min. Use Autograph to measure the stress (N / cm) at this time. The force sensor of Autograph uses 1N.
[0212] (Maximum test force)
[0213] The bending strength (bending strength, three-point bending test) is measured by the method according to ASTM D790. The negative electrode with negative electrode material layers on both sides is cut into 15mm×20mm size to prepare a test piece. Using the three-point bending method, the test piece is arranged between the first and second locations with an interval of 10mm, and a probe is used to press the middle of the test piece (third location) at a constant speed along the thickness direction of the test piece to perform a bending test (bending property test). While moving at a speed of 5mm / min in the thickness direction of the third location, the applied force is measured. The maximum bending strength (maximum bending force or maximum bending strength) is the maximum value of the force applied to the test piece according to the moving distance of the probe.
[0214] (Preparation of Electrolyte)
[0215] Ethylene carbonate as a high dielectric constant solvent and ethyl methyl carbonate as a low viscosity solvent are mixed in a volume ratio of 30:70, LiPF6 is added thereto to give a concentration of 1.0 mol / L, and 2 mass % of vinylene carbonate is added thereto to obtain a non-aqueous electrolyte.
[0216] (Production of positive electrode)
[0217] Add LiNi as the positive electrode active material 0.6 Mn 0.2 Co 0.2 97 parts by mass of O2 (NMC622), 1.5 parts by mass of acetylene black (AB) as a conductive aid, and 1.5 parts by mass of polyvinylidene fluoride (8% by mass NMP solution) as a binder were mixed with a disperser to form a slurry. The obtained slurry was applied to an aluminum foil with a thickness of 20 μm and dried, and rolled with a press. The obtained product was cut into a shape having a coated portion (positive electrode material layer) with a width of 50 mm and a length of 30 mm and an uncoated portion with a width of 5 mm and a length of 9 mm as a positive electrode.
[0218] (Manufacturing of lithium-ion secondary batteries)
[0219] The negative electrodes prepared in Examples and Comparative Examples and having a negative electrode material layer on one surface were cut into a shape having a coated portion (negative electrode material layer) of 52 mm in width and 32 mm in length and an uncoated portion of 5 mm in width and 9 mm in height to prepare negative electrodes.
[0220] The positive electrode and the negative electrode are placed opposite to each other with a microporous polyethylene film (diaphragm) having a thickness of 20 μm between them, and the non-aqueous electrolyte obtained above is injected. After the non-aqueous electrolyte fully permeates the diaphragm, etc., it is sealed and pre-charged and aged to produce an aluminum laminate battery (lithium-ion secondary battery).
[0221] (Measurement of battery characteristics)
[0222] The obtained aluminum laminate battery was examined for the cycle capacity maintenance rate and gas increase rate at 45° C. as described below.
[0223] (Cycle Characteristics)
[0224] The obtained aluminum laminate battery was charged at 25°C with a constant current-constant voltage (hereinafter referred to as CC / CV charging) to 4.2V (0.1C cutoff) at a current equivalent to 0.2C, and then discharged to 3V at a constant current of 0.2C, which was regarded as one cycle, and three cycles were performed. Then, CC / CV charging (0.1C cutoff) was performed at 45°C with a current equivalent to 1.0C to 4.2V, and then discharged to 3V at a constant current of 1.0C, which was regarded as one cycle, and the initial discharge capacity was calculated from the discharge capacity. The cycle was repeated again, and the discharge capacity after 300 cycles was measured. The ratio of the discharge capacity after 300 cycles to the initial discharge capacity was calculated and used as the capacity retention rate (%).
[0225] Capacity retention rate (%) = (discharge capacity after 300 cycles) ÷ (initial discharge capacity at 1.0C) × 100
[0226] (Determination of gas increase rate)
[0227] The volume of the battery after the evaluation of the cycle characteristics was completed was measured by the Archimedean method, and the gas increase rate was calculated from the volume change before and after charge and discharge.
[0228] Gas increase rate (%) = (volume after 300 cycles (ml)) / (initial volume (ml)) × 100
[0229] The above results are shown in Tables 1 and 2.
[0230]
[0231]
Claims
1. A negative electrode mixture, comprising single-walled carbon nanotubes, a negative electrode active material and a binder, wherein: The negative electrode active material includes a negative electrode active material which exhibits a potential of 2.5 V or less based on Li when alloyed with Li or combined with Li, The binder contains a fluorine-containing copolymer containing vinylidene fluoride units and other monomer units other than vinylidene fluoride.
2. The negative electrode mixture according to claim 1, wherein The negative electrode active material is a compound containing at least one element selected from the group consisting of Si, Sn, V, Nb and Ti.
3. The negative electrode mixture according to claim 1, wherein The negative electrode active material is selected from Si and SiO x At least one of the groups consisting of <x<2。 4. The negative electrode mixture according to claim 1, wherein The negative electrode active material is a carbonaceous material.
5. The negative electrode mixture according to claim 1, wherein The negative electrode active material is a compound containing at least one element selected from the group consisting of Si, Sn, V, Nb and Ti, and a carbonaceous material.
6. The negative electrode mixture according to any one of claims 1 to 5, wherein The average outer diameter of the single-walled carbon nanotube is less than 2.5 nm.
7. The negative electrode mixture according to any one of claims 1 to 6, wherein The average G / D ratio of the single-walled carbon nanotubes is 2 or more.
8. The negative electrode mixture according to any one of claims 1 to 7, wherein The content of the single-walled carbon nanotubes is 0.001% by mass to 10% by mass based on the solid content mass of the negative electrode mixture.
9. The negative electrode mixture according to any one of claims 1 to 8, wherein The other monomers are fluorinated monomers, wherein the fluorinated monomers do not include vinylidene fluoride units.
10. The negative electrode mixture according to any one of claims 1 to 8, wherein The other monomer is at least one selected from the group consisting of tetrafluoroethylene, chlorotrifluoroethylene, (meth)acrylic acid, 2,3,3,3-tetrafluoropropylene, hexafluoropropylene, and fluoroalkyl vinyl ether.
11. The negative electrode mixture according to any one of claims 1 to 10, wherein The binder further contains polyvinylidene fluoride.
12. The negative electrode mixture according to claim 11, wherein The mass ratio of the polyvinylidene fluoride to the fluorine-containing copolymer, that is, polyvinylidene fluoride / fluorine-containing copolymer is 99 / 1 to 1 / 99. 13 . The negative electrode mixture according to claim 1 , further comprising a solvent.
14. A negative electrode, comprising: a current collector; and A negative electrode material layer is provided on one side or both sides of the current collector and is formed of the negative electrode mixture according to any one of claims 1 to 13. 15 . A secondary battery comprising the negative electrode according to claim 14 .
Citation Information
Patent Citations
Secondary battery, battery pack, electric vehicle, electric tool and electronic device
WO2018146865A1