Application of catalyst in reaction of catalyzing CO in mixed gas to reduce NO

By using Pt and Ni single-atom alloy catalysts supported by TiO2 nanosheets in automobile exhaust purification catalysts, the problems of high precious metal loading and insufficient catalytic activity are solved, and high-efficiency catalytic activity and high stability of the CO reduction NO reaction are achieved, reducing the The amount of precious metals used.

CN118847142AActive Publication Date: 2024-10-29DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310472115.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-10-29
Estimated Expiration
2043-04-27

AI Technical Summary

Technical Problem

The precious metals such as Pt, Pd, and Rh used in existing automobile exhaust purification catalysts have high loadings, resulting in high costs. It is difficult to effectively reduce the amount of precious metals with existing technology, and at the same time, the catalytic activity is insufficient in the CO reduction NO reaction.

Method used

TiO2 nanosheets are used to load Pt and Ni single-atom alloy catalysts. TiO2 nanosheets are synthesized by hydrothermal method and calcined in a hydrogen atmosphere to form a supported catalyst to ensure the dispersed state of single atoms of Pt and Ni and improve catalytic activity.

Benefits of technology

The highly efficient catalytic activity and N2 selectivity of the CO reduction NO reaction are achieved. The N2 selectivity in the product is greater than 90%. At the same time, the catalyst has high stability and reduces the amount of precious metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004204403470000011
    Figure HDA0004204403470000011
Patent Text Reader

Abstract

The invention belongs to the technical field of chemical engineering, and relates to a monatomic alloy catalyst with platinum and nickel bimetals loaded on anatase-phase titanium dioxide nanosheets, which is used for reducing nitric oxide from carbon monoxide in an automobile exhaust purification reaction. The catalyst takes TiO2 as a main body and is loaded with Pt and Ni monatomic alloy. The catalyst is applied to a reaction of reducing NO by CO, and has good low-temperature activity and selectivity of a target product N2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to application of a TiO2 nanosheet-loaded Pt and Ni single-atom alloy catalyst in the reaction of reducing NO with CO in automobile tail gas purification. Background Art

[0002] In recent years, with the development of social economy and science and technology, the number of motor vehicles has shown explosive growth. The harm of automobile exhaust to the environment and people is becoming more and more serious. And NO in exhaust gas will cause environmental problems such as acid rain, ozone hole, photochemical smog, etc., which seriously threatens human health. Therefore, the requirements for automobile exhaust purification are getting higher and higher. How to efficiently purify NO in exhaust gas has become an urgent problem to be solved.

[0003] The three-way catalysts currently used commercially mainly use high-load Pt, Pd, Rh and other precious metals as active ingredients, and the precious metals are expensive, which makes the cost of three-way catalysts very high. Therefore, the demand for reducing the precious metal loading is becoming more and more urgent. The development of low-precious metal catalysts is an inevitable trend. Single atoms have attracted widespread attention because they can maximize the atomic utilization rate and show catalytic activity that particle catalysts do not have. Therefore, whether it is possible to synthesize single-atom alloy catalysts, while ensuring that the precious metals are dispersed in single atoms, and change the properties of the active center through the synergistic effect of the two metals that form the alloy, can not only greatly improve the catalytic activity, but also effectively reduce the amount of precious metals. Summary of the invention

[0004] One object of the present invention is to provide a TiO2 nanosheet-loaded Pt, Ni single-atom alloy catalyst.

[0005] The second object of the present invention is to provide a method for preparing TiO2 nanosheet-loaded Pt, Ni single-atom alloy catalyst.

[0006] The third object of the present invention is to provide an application of TiO2 nanosheets loaded with Pt, Ni single atom alloy catalyst.

[0007] To achieve the above object, the present invention provides a TiO2 nanosheet-loaded Pt, Ni single-atom alloy catalyst, the preparation method of which comprises the following steps:

[0008] 1) Synthesis of anatase TiO2 nanosheets;

[0009] The synthesis of the nanosheets consists of a titanium source and an acid, wherein the molar ratio of the acid to the titanium source is 0.5-2. After being stirred evenly, the mixture is transferred to a polytetrafluoroethylene liner, and the liner is placed in a hydrothermal autoclave. After high-temperature crystallization, the product is centrifuged, washed with deionized water and ethanol, and then dried to obtain TiO2 nanosheets.

[0010] Preferably, the molar ratio of acid to titanium source is 0.8-1.

[0011] Preferably, the titanium source is tetrabutyl titanate or tetraisopropyl titanate.

[0012] Preferably, the acid is hydrofluoric acid.

[0013] Preferably, the high temperature crystallization temperature is 180-200° C., and the crystallization time is 20-36 hours. More preferably, the crystallization temperature is 200° C., and the crystallization time is 24 hours.

[0014] 2) Synthesis of TiO2-supported Pt and Ni single-atom alloy catalysts;

[0015] The precursors of Pt and Ni are dissolved in water and mixed evenly with the prepared TiO2 nanosheets. The mixed slurry is freeze-dried, calcined in a muffle furnace, and reduced in a hydrogen atmosphere to obtain a TiO2-loaded Pt and Ni single-atom alloy catalyst.

[0016] Preferably, the Pt precursor is chloroplatinic acid, and the Ni precursor is nickel nitrate or nickel acetate.

[0017] Preferably, the concentration of the Pt precursor is: 5 mmol·L -1 -50mmol·L -1 More preferably, the concentration of the Pt precursor is: 20 mmol·L -1 -30mmol·L -1 .

[0018] Preferably, the concentration of Ni precursor is: 680mmol·L -1 -1700mmol·L -1 More preferably, the concentration of Ni precursor is: 850mmol·L -1 -1200mmol·L -1 .

[0019] Preferably, the calcination temperature is 400-500° C. and the calcination time is 2-3 hours.

[0020] Preferably, the reduction hydrogen concentration is 5%-100%, the reduction temperature is 400-500°C, and the reduction time is 1-3h.

[0021] For the supported catalyst provided by the present invention, the catalytic activity test method is as follows:

[0022] Add granulated catalyst to the fixed bed, reduce in hydrogen atmosphere for 2-3 hours, cool to room temperature, introduce mixed gas of CO, NO (concentration is 0.1%-0.5%, He is the balance gas), the reaction procedure is: maintain at 50℃ for 30min, increase to 100℃ for 30min, increase to 150℃ for 30min, increase to 200℃ for 30min, increase to 250℃ for 30min, increase to 300℃ for 30min, increase to 350℃ for 30min, increase to 400℃ for 30min. Detect the concentration of products in the tail gas by chromatography.

[0023] The catalyst is used in the reaction of CO reducing NO and has good low-temperature activity and selectivity for the target product N2.

[0024] The present invention has the following effects:

[0025] 1. The preparation process of the supported noble metal catalyst is simple and easy to control. The active metal in the prepared catalyst is highly dispersed in the form of a single-atom alloy;

[0026] 2. The prepared catalyst has good catalytic activity and selectivity in the CO reduction of NO reaction, the selectivity of N2 in the product is greater than 90%, and it has high stability. Description of the drawings:

[0027] Figure 1 is a high-angle annular dark field image of a single-atom alloy catalyst in an embodiment; DETAILED DESCRIPTION

[0028] Embodiment 1:

[0029] 1) 10 ml of tetrabutyl titanate and 1.0 ml of hydrofluoric acid (40 wt%, AR) were mixed in a hydrothermal reactor and hydrothermally reacted at 200°C for 20 h. The solid product was washed with deionized water and ethanol in turn and dried at 60°C for 8 h to obtain anatase phase TiO2 nanosheets with a size of about 2000-3000 nm. 2 , thickness is about 10-20nm. 2) Take 0.011g chloroplatinic acid and 0.248g nickel nitrate and dissolve them in 1ml water, add them to 1g TiO2 nanosheets, stir and freeze-dry, calcine at 400℃ for 2h, and reduce them in a 5% volume concentration hydrogen atmosphere (He gas balance) for 2h. Electron microscope photos show that a catalyst of TiO2 loaded Pt and Ni single atom alloy is obtained. Characterized by HAADF-STEM, Pt is uniformly dispersed on the second metal component Ni in the form of single atoms, and the Ni particle size is between 4-10nm.

[0030] Embodiment 2:

[0031] 1) 12.5 ml of tetrabutyl titanate and 3 ml of hydrofluoric acid (40 wt%, AR) were mixed in a hydrothermal reactor and hydrothermally reacted at 200°C for 20 h. The solid product was washed with deionized water and ethanol in turn and dried at 60°C for 8 h to obtain anatase phase TiO2 nanosheets with a size of about 2000-3000 nm. 2 , with a thickness of about 10-20nm. 2) Take 0.011g of chloroplatinic acid and 0.248g of nickel nitrate and dissolve them in 1ml of water, add them to 1g of TiO2 nanosheets, stir and freeze-dry, calcine at 400℃ for 2h, and reduce them for 2h in a 5% volume concentration hydrogen atmosphere (He gas balance). Electron microscope photos show that a catalyst of TiO2-loaded Pt and Ni single-atom alloy is obtained. According to HAADF-STEM characterization, Pt is uniformly dispersed on the second metal component Ni in the form of single atoms, and the Ni particle size is between 4-10nm.

[0032] Embodiment 3:

[0033] 1) Mix 25 ml of tetrabutyl titanate and 3 ml of hydrofluoric acid (40 wt%, AR) in a hydrothermal reactor and perform hydrothermal reaction at 200°C for 20 h. The solid product is washed with deionized water and ethanol in turn and dried at 60°C for 8 h to obtain anatase phase TiO2 nanosheets with a size of about 2000-3000 nm. 2 , with a thickness of about 10-20nm.

[0034] 2) Take 0.011g chloroplatinic acid and 0.248g nickel nitrate and dissolve them in 1ml water, add them to 1g TiO2 nanosheets, stir and freeze-dry, calcine at 400℃ for 2h, and reduce them for 2h in a 5% volume concentration hydrogen atmosphere (He gas balance). Electron microscope photos show that a catalyst of TiO2-loaded Pt and Ni single-atom alloy is obtained. HAADF-STEM characterization shows that Pt is uniformly dispersed on the second metal component Ni in the form of single atoms, and the Ni particle size is between 4-10nm.

[0035] Embodiment 4:

[0036] 1) 10 ml of tetrabutyl titanate and 1.0 ml of hydrofluoric acid (40 wt%, AR) were mixed in a hydrothermal reactor and hydrothermally reacted at 200°C for 20 h. The solid product was washed with deionized water and ethanol in turn and dried at 60°C for 8 h to obtain anatase phase TiO2 nanosheets with a size of about 2000-3000 nm. 2, with a thickness of about 10-20nm. 2) Take 0.011g of chloroplatinic acid and 0.496g of nickel nitrate and dissolve them in 1ml of water, add them to 1g of TiO2 nanosheets, stir and freeze-dry, calcine at 400℃ for 2h, and reduce them for 2h in a 5% volume concentration hydrogen atmosphere (He gas balance). Electron microscopy photos show that a catalyst of TiO2-loaded Pt and Ni single-atom alloy is obtained. According to HAADF-STEM characterization, Pt is uniformly dispersed on the second metal component Ni in the form of single atoms, and the Ni particle size is between 4-10nm.

[0037] Embodiment 5:

[0038] 1) 12.5 ml of tetrabutyl titanate and 3 ml of hydrofluoric acid (40 wt%, AR) were mixed in a hydrothermal reactor and hydrothermally reacted at 200°C for 20 h. The solid product was washed with deionized water and ethanol in turn and dried at 60°C for 8 h to obtain anatase phase TiO2 nanosheets with a size of about 2000-3000 nm. 2 , with a thickness of about 10-20nm. 2) Take 0.011g of chloroplatinic acid and 0.496g of nickel nitrate and dissolve them in 1ml of water, add them to 1g of TiO2 nanosheets, stir and freeze-dry, calcine at 400℃ for 2h, and reduce them for 2h in a 5% volume concentration hydrogen atmosphere (He gas balance). Electron microscopy photos show that a catalyst of TiO2-loaded Pt and Ni single-atom alloy is obtained. According to HAADF-STEM characterization, Pt is uniformly dispersed on the second metal component Ni in the form of single atoms, and the Ni particle size is between 4-10nm.

[0039] Embodiment 6:

[0040] 1) Mix 25 ml of tetrabutyl titanate and 3 ml of hydrofluoric acid (40 wt%, AR) in a hydrothermal reactor and perform hydrothermal reaction at 200°C for 20 h. The solid product is washed with deionized water and ethanol in turn and dried at 60°C for 8 h to obtain anatase phase TiO2 nanosheets with a size of about 2000-3000 nm. 2 , with a thickness of about 10-20nm.

[0041] 2) Take 0.011g chloroplatinic acid and 0.496g nickel nitrate and dissolve them in 1ml water, add them to 1g TiO2 nanosheets, stir and freeze-dry, calcine at 400℃ for 2h, and reduce them for 2h in a 5% hydrogen atmosphere (He gas balance). Electron microscope photos show that a catalyst of TiO2-loaded Pt and Ni single-atom alloy is obtained. HAADF-STEM characterization shows that Pt is uniformly dispersed on the second metal component Ni in the form of single atoms, and the Ni particle size is between 4-10nm.

[0042] Embodiment 7:

[0043] 1) 10 ml of tetrabutyl titanate and 1.0 ml of hydrofluoric acid (40 wt%, AR) were mixed in a hydrothermal reactor and hydrothermally reacted at 180°C for 36 h. The solid product was washed with deionized water and ethanol in turn and dried at 60°C for 8 h to obtain anatase phase TiO2 nanosheets with a size of about 2000-3000 nm. 2 , with a thickness of about 10-20nm. 2) Take 0.011g of chloroplatinic acid and 0.248g of nickel nitrate and dissolve them in 1ml of water, add them to 1g of TiO2 nanosheets, stir and freeze-dry, calcine at 400℃ for 2h, and reduce them for 2h in a 5% volume concentration hydrogen atmosphere (He gas balance). Electron microscope photos show that a catalyst of TiO2-loaded Pt and Ni single-atom alloy is obtained. According to HAADF-STEM characterization, Pt is uniformly dispersed on the second metal component Ni in the form of single atoms, and the Ni particle size is between 4-10nm.

[0044] Embodiment 8:

[0045] 1) 12.5 ml of tetrabutyl titanate and 3 ml of hydrofluoric acid (40 wt%, AR) were mixed in a hydrothermal reactor and hydrothermally reacted at 180°C for 36 h. The solid product was washed with deionized water and ethanol in turn and dried at 60°C for 8 h to obtain anatase phase TiO2 nanosheets with a size of about 2000-3000 nm. 2 , with a thickness of about 10-20nm.

[0046] 2) Take 0.011g chloroplatinic acid and 0.248g nickel nitrate and dissolve them in 1ml water, add them to 1g TiO2 nanosheets, stir and freeze-dry, calcine at 400℃ for 2h, and reduce them for 2h in a 5% volume concentration hydrogen atmosphere (He gas balance). Electron microscope photos show that a catalyst of TiO2-loaded Pt and Ni single-atom alloy is obtained. HAADF-STEM characterization shows that Pt is uniformly dispersed on the second metal component Ni in the form of single atoms, and the Ni particle size is between 4-10nm.

[0047] Embodiment 9:

[0048] 1) Mix 25 ml of tetrabutyl titanate and 3 ml of hydrofluoric acid (40 wt%, AR) in a hydrothermal reactor and perform hydrothermal reaction at 180°C for 36 h. The solid product is washed with deionized water and ethanol in turn and dried at 60°C for 8 h to obtain anatase phase TiO2 nanosheets with a size of about 2000-3000 nm. 2 , with a thickness of about 10-20nm.

[0049] 2) Take 0.011g chloroplatinic acid and 0.248g nickel nitrate and dissolve them in 1ml water, add them to 1g TiO2 nanosheets, stir and freeze-dry, calcine at 400℃ for 2h, and reduce them for 2h in a 5% volume concentration hydrogen atmosphere (He gas balance). Electron microscope photos show that a catalyst of TiO2-loaded Pt and Ni single-atom alloy is obtained. HAADF-STEM characterization shows that Pt is uniformly dispersed on the second metal component Ni in the form of single atoms, and the Ni particle size is between 4-10nm.

[0050] Application Example 1:

[0051] 100 mg of the catalyst prepared in Example 1 was granulated into 40-60 mesh, added to a quartz tube of a fixed bed, and fed with 0.2% CO, 0.2% NO reaction gas (He gas balance, volume space velocity of 20000 ml / (g*h)). The reaction procedure was: 50°C for 30 min, raised to 100°C for 30 min, raised to 150°C for 30 min, raised to 200°C for 30 min, raised to 250°C for 30 min, raised to 300°C for 30 min, raised to 350°C for 30 min, raised to 400°C for 30 min. The tail gas was passed into a chromatographic analysis, and it began to be active at 100°C, at which time the NO conversion rate was 15%, and the CO conversion rate was 11%. At 150°C, the NO conversion rate was 37%, and the CO conversion rate was 32%. At 200°C, the NO conversion rate was 75%, and the CO conversion rate was 72%. Above 250°C up to 400°C, NO is completely converted, the N2 selectivity in the NO conversion product is 95%, and only a small amount of by-product N2O exists.

[0052] Application Example 2:

[0053] 100 mg of the catalyst prepared in Example 2 was granulated into 40-60 mesh, added to a quartz tube of a fixed bed, and fed with 0.2% CO, 0.2% NO reaction gas (He gas balance, volume space velocity of 20000 ml / (g*h)), the reaction procedure was: 50°C for 30 min, raised to 100°C for 30 min, raised to 150°C for 30 min, raised to 200°C for 30 min, raised to 250°C for 30 min, raised to 300°C for 30 min, raised to 350°C for 30 min, raised to 400°C for 30 min. The tail gas was passed into a chromatographic analysis, and it began to be active at 100°C, at which time the NO conversion rate was 14%, and the CO conversion rate was 9%. At 150°C, the NO conversion rate was 38%, and the CO conversion rate was 34%. At 200°C, the NO conversion rate was 76%, and the CO conversion rate was 73%. Above 250°C up to 400°C, NO is completely converted, the N2 selectivity in the product is 94%, and only a small amount of by-product N2O is present.

[0054] Application Example 3:

[0055] 100 mg of the catalyst prepared in Example 3 was granulated into 40-60 mesh, added to a quartz tube of a fixed bed, and a reaction gas of 0.2% CO and 0.2% NO (He gas balance, volume space velocity of 20000 ml / (g*h)) was introduced. The reaction procedure was: 50°C for 30 min, raised to 100°C for 30 min, raised to 150°C for 30 min, raised to 200°C for 30 min, raised to 250°C for 30 min, raised to 300°C for 30 min, raised to 350°C for 30 min, raised to 400°C for 30 min. The tail gas was passed into a chromatographic analysis, and it began to be active at 100°C, at which time the NO conversion rate was 15%, and the CO conversion rate was 10%. At 150°C, the NO conversion rate was 40%, and the CO conversion rate was 35%. At 200°C, the NO conversion rate was 77%, and the CO conversion rate was 74%. Above 250°C up to 400°C, NO is completely converted, with N2 selectivity of 95% in the product and only a small amount of by-product N2O.

[0056] Application Example 4:

[0057] 100 mg of the catalyst prepared in Example 4 was granulated into 40-60 mesh, added to the quartz tube of the fixed bed, and passed through the reaction gas of 0.2% CO and 0.2% NO (He gas balance, volume space velocity is 20000 ml / (g*h)). The reaction procedure is: maintain at 50°C for 30 minutes, increase to 100°C for 30 minutes, increase to 150°C for 30 minutes, increase to 200°C for 30 minutes, increase to 250°C for 30 minutes, increase to 300°C for 30 minutes, increase to 350°C for 30 minutes, increase to 400°C for 30 minutes. The tail gas was passed into the chromatographic analysis, and it began to be active at 100°C, at which time the NO conversion rate was 7%, and the CO conversion rate was 3%. At 150°C, the NO conversion rate was 30%, and the CO conversion rate was 24%. At 200°C, the NO conversion rate was 66%, and the CO conversion rate was 60%. . At temperatures above 250°C up to 400°C, the NO conversion rate is 90%, and the CO conversion rate is 88%. The N2 selectivity in the product is 85%, and the remaining product is the by-product N2O.

[0058] Application Example 5:

[0059] 100 mg of the catalyst prepared in Example 5 was granulated into 40-60 mesh, added to a quartz tube of a fixed bed, and a reaction gas of 0.2% CO and 0.2% NO (He gas balance, volume space velocity of 20000 ml / (g*h)) was introduced. The reaction procedure was: 50°C for 30 min, raised to 100°C for 30 min, raised to 150°C for 30 min, raised to 200°C for 30 min, raised to 250°C for 30 min, raised to 300°C for 30 min, raised to 350°C for 30 min, raised to 400°C for 30 min. The tail gas was passed into a chromatographic analysis, and it began to be active at 100°C, at which time the NO conversion rate was 8%, and the CO conversion rate was 4%. At 150°C, the NO conversion rate was 31%, and the CO conversion rate was 24%. At 200°C, the NO conversion rate was 70%, and the CO conversion rate was 65%. At temperatures above 250°C up to 400°C, the NO conversion rate is 92%, and the CO conversion rate is 90%. The N2 selectivity in the product is 87%, and the remaining product is the by-product N2O.

[0060] Application Example 6:

[0061] 100 mg of the catalyst prepared in Example 6 was granulated into 40-60 mesh, added to a quartz tube of a fixed bed, and fed with 0.2% CO, 0.2% NO reaction gas (He gas balance, volume space velocity of 20000 ml / (g*h)). The reaction procedure was: 50°C for 30 min, raised to 100°C for 30 min, raised to 150°C for 30 min, raised to 200°C for 30 min, raised to 250°C for 30 min, raised to 300°C for 30 min, raised to 350°C for 30 min, raised to 400°C for 30 min. The tail gas was passed into a chromatographic analysis, and it began to be active at 100°C, at which time the NO conversion rate was 7%, and the CO conversion rate was 5%. At 150°C, the NO conversion rate was 35%, and the CO conversion rate was 30%. At 200°C, the NO conversion rate was 71%, and the CO conversion rate was 66%. At temperatures above 250°C up to 400°C, the NO conversion rate is 92%, and the CO conversion rate is 91%. The N2 selectivity in the product is 88%, and the remaining product is the by-product N2O.

[0062] Application Example 7:

[0063] 100 mg of the catalyst prepared in Example 7 was granulated into 40-60 mesh, added to a quartz tube of a fixed bed, and fed with 0.2% CO, 0.2% NO reaction gas (He gas balance, volume space velocity of 20000 ml / (g*h)). The reaction procedure was: 50°C for 30 min, raised to 100°C for 30 min, raised to 150°C for 30 min, raised to 200°C for 30 min, raised to 250°C for 30 min, raised to 300°C for 30 min, raised to 350°C for 30 min, raised to 400°C for 30 min. The tail gas was passed into a chromatographic analysis, and it began to be active at 100°C, at which time the NO conversion rate was 16%, and the CO conversion rate was 10%. At 150°C, the NO conversion rate was 38%, and the CO conversion rate was 32%. At 200°C, the NO conversion rate was 76%, and the CO conversion rate was 71%. At temperatures above 250°C up to 400°C, NO is completely converted, with N2 selectivity of 97% in the product and only a small amount of by-product N2O.

[0064] Application Example 8:

[0065] 100 mg of the catalyst prepared in Example 8 was granulated into 40-60 mesh, added to a quartz tube of a fixed bed, and a reaction gas of 0.2% CO and 0.2% NO (He gas balance, volume space velocity of 20000 ml / (g*h)) was introduced. The reaction procedure was: 50°C for 30 min, raised to 100°C for 30 min, raised to 150°C for 30 min, raised to 200°C for 30 min, raised to 250°C for 30 min, raised to 300°C for 30 min, raised to 350°C for 30 min, and raised to 400°C for 30 min. The tail gas was passed into a chromatographic analysis, and it began to be active at 100°C, at which time the NO conversion rate was 17%, and the CO conversion rate was 14%. At 150°C, the NO conversion rate was 41%, and the CO conversion rate was 37%. At 200°C, the NO conversion rate was 79%, and the CO conversion rate was 74%. At temperatures above 250°C up to 400°C, NO is completely converted, with N2 selectivity of 94% in the product and only a small amount of by-product N2O.

[0066] Application Example 9:

[0067] 100 mg of the catalyst prepared in Example 9 was granulated into 40-60 mesh, added to a quartz tube of a fixed bed, and fed with 0.2% CO, 0.2% NO reaction gas (He gas balance, volume space velocity of 20000 ml / (g*h)). The reaction procedure was: 50°C for 30 min, raised to 100°C for 30 min, raised to 150°C for 30 min, raised to 200°C for 30 min, raised to 250°C for 30 min, raised to 300°C for 30 min, raised to 350°C for 30 min, raised to 400°C for 30 min. The tail gas was passed into a chromatographic analysis, and it began to be active at 100°C, at which time the NO conversion rate was 14%, and the CO conversion rate was 11%. At 150°C, the NO conversion rate was 38%, and the CO conversion rate was 33%. At 200°C, the NO conversion rate was 77%, and the CO conversion rate was 74%. At temperatures above 250°C up to 400°C, NO is completely converted, with N2 selectivity of 93% in the product and only a small amount of by-product N2O.

[0068] Comparative Example 1:

[0069] Take 100mg TiO2 loaded with Pt nanoparticles catalyst (prepared by equal volume impregnation method, loading of 0.5%, named Pt NP-TiO2), the Pt particle size is between 0.4nm-1.4nm. The catalyst is granulated into 40-60 mesh, added to the quartz tube of the fixed bed, and passed into 0.2% CO, 0.2% NO reaction gas (He gas balance, volume space velocity is 20000ml / (g*h)), the reaction procedure is: 50℃ for 30min, rise to 100℃ for 30min, rise to 150℃ for 30min, rise to 200℃ for 30min, rise to 250℃ for 30min, rise to 300℃ for 30min, rise to 350℃ for 30min, rise to 400℃ for 30min. The tail gas is passed into the chromatographic analysis, and it starts to be active at 150℃, at which time the NO conversion rate is 5% and the CO conversion rate is 4%. At 200℃ to 300℃, the NO conversion rate is 10% and the CO conversion rate is 8%. At 350℃, the NO conversion rate is 25% and the CO conversion rate is 21%. At 400℃, the NO conversion rate is 59% and the CO conversion rate is 55%. At this time, the N2 selectivity in the product is 39%, and the remaining product is the by-product N2O.

[0070] Comparative Example 2:

[0071] Take 100mg TiO2 loaded Ni nanoparticle catalyst (prepared by equal volume impregnation method, loading is 5%, named Ni NP-TiO2), Ni particle size is between 10-27nm, the catalyst is granulated into 40-60 mesh, added to the fixed bed quartz tube, and passed into 0.2% CO, 0.2% NO reaction gas (He gas balance, volume space velocity is 20000ml / (g*h)), the reaction procedure is: 50℃ for 30min, rise to 100℃ for 30min, rise to 150℃ for 30min, rise to 200℃ for 30min, rise to 250℃ for 30min, rise to 300℃ for 30min, rise to 350℃ for 30min, rise to 400℃ for 30min. The tail gas is passed into the chromatographic analysis, during the reaction process, the NO conversion rate is 0%, and the CO conversion rate is 0%. The N2 selectivity in the product is 0%.

[0072] Comparative Example 3:

[0073] Take 100mg TiO2 loaded with Pt, Ni common alloy nanoparticles catalyst (prepared by equal volume impregnation method, Pt loading is 0.5%, Ni loading is 0.5%. Named PtNi NP-TiO2), Pt, Ni form common alloy, particle size is between 4-10nm. The catalyst is granulated into 40-60 mesh, added to the quartz tube of the fixed bed, and 0.2% CO, 0.2% NO reaction gas (He gas balance, volume space velocity is 20000ml / (g*h)) is introduced. The reaction procedure is: 50℃ for 30min, raised to 100℃ for 30min, raised to 150℃ for 30min, raised to 200℃ for 30min, raised to 250℃ for 30min, raised to 300℃ for 30min, raised to 350℃ for 30min, raised to 400℃ for 30min. The tail gas was passed through the chromatographic analysis, and there was almost no activity at 50℃ to 200℃. At 250℃, the NO conversion rate was 25%, and the CO conversion rate was 23%. At 300℃, the NO conversion rate was 80%, and the CO conversion rate was 74%. At 350℃ to 400℃, the NO conversion rate was 85%, and the CO conversion rate was 80%. At this time, the N2 selectivity in the product was 41%, and the rest of the product was the by-product N2O.

[0074] Results Analysis

[0075] According to the comparison between Application Examples 1-9 and Comparative Example 1, the catalytic activity of Pt and Ni alloy is significantly better than that of the single Pt catalyst, indicating that Pt and Ni have a significant synergistic promoting effect on the reaction.

[0076] According to the comparison between Application Examples 1-9 and Comparative Example 2, the single Ni catalyst itself is inactive, but adding a small amount of Pt to Ni can greatly improve the catalytic activity, which shows that Pt is an essential active component in this reaction, while Ni is an excellent auxiliary agent.

[0077] According to the comparison between Application Examples 1-9 and Comparative Example 3, the performance of Pt, Ni single-atom alloy catalyst is significantly better than that of Pt, Ni ordinary alloy catalyst. This shows the advantage of single atoms in this reaction. Pt, Ni form single-atom alloys, and due to the unique electronic effect between bimetallic metals, the electron density of Pt is changed, which effectively improves the conversion rate of NO and the selectivity of N2.

Claims

1. Use of a catalyst in catalyzing the reduction of NO by CO in a mixed gas, characterized in that: The catalyst uses TiO2 as a carrier and loads Pt and Ni as main active components; the loading amount of Pt relative to the carrier is 0.1-1wt% of the carrier (preferably, the loading amount is 0.1-0.7wt%, more preferably, the loading amount is 0.4-0.6wt%), and the loading amount of Ni relative to the carrier is 4-10wt% (preferably, the loading amount is 4-8wt%, more preferably, the loading amount is 4-6wt%).

2. The use according to claim 1, characterized in that The mixed gas is a mixed gas containing CO and NO, preferably automobile exhaust gas.

3. The use according to claim 1, characterized in that: Pt is uniformly dispersed on the second metal component Ni in the form of single atoms, the Ni particle size is between 4-10nm, and the Ni particles are loaded on the TiO2 carrier.

4. The use according to claim 1 or 3, characterized in that: Pt and Ni form a single-atom alloy; the TiO2 carrier is anatase phase TiO2 nanosheets.

5. The use according to any one of claims 1 to 4, characterized in that: The preparation process of the catalyst is as follows: 1) Synthesis of anatase TiO2 nanosheets; The synthesis of the nanosheets consists of a titanium source and an acid, wherein the molar ratio of the acid to the titanium source is 0.5-2 (preferably, the molar ratio of the acid to the titanium source is 0.7-1.5; more preferably, the molar ratio of the acid to the titanium source is 1.2-1.5); the titanium source and the acid are mixed and stirred evenly and then placed in a hydrothermal kettle for high-temperature crystallization. After the high-temperature crystallization is completed, the product is centrifuged and the solid product is dried to obtain TiO2 nanosheets; the crystallization temperature is 180-200°C (preferably, the crystallization temperature is 190-200°C; more preferably, the crystallization temperature is 200°C), and the crystallization time is 20-36 hours (preferably, the crystallization time is 24-36 hours; more preferably, the crystallization time is 24 hours); 2) Synthesis of TiO2-loaded Pt and Ni catalysts; The precursors of Pt and Ni are dissolved in water and mixed evenly with the prepared TiO2 nanosheets. The mixed slurry is freeze-dried and then calcined in a muffle furnace at 400-500°C for 2-3h (preferably 400°C for 2 hours). Before the reaction, it is reduced at 400°C for 1-2h (preferably 5% hydrogen, balanced by He gas, for 2 hours) in an atmosphere containing 5%-100% hydrogen by volume (the remaining gas is one or more of He gas or Ar gas) to obtain a TiO2-loaded Pt and Ni catalyst.

6. The use according to claim 5, characterized in that: The titanium source used is tetrabutyl titanate or tetraisopropyl titanate, preferably, the titanium source is tetrabutyl titanate; The acid is hydrofluoric acid with a mass concentration of 30%-40%, preferably, 40% hydrofluoric acid is selected.

7. The method for preparing a catalyst of TiO2-loaded Pt, Ni single-atom alloy according to claim 5, characterized in that: The Pt source was chloroplatinic acid; The Ni source is nickel nitrate and / or nickel acetate. Preferably, the Ni source is nickel nitrate.

8. The use according to any one of claims 1 to 7, characterized in that: The specific reaction process is: in a fixed bed, add a catalyst (preferably with a particle size of 40-60 mesh, more preferably with a particle size of 40-50 mesh), 5-15% volume fraction hydrogen (helium balance, preferably, the volume fraction of hydrogen is 5-10%, more preferably, the volume fraction of hydrogen is 5%), reduce at 400°C-500°C for 1-2 hours (preferably, the reduction temperature is 400°C-450°C, the reduction time is 1.5-2h, more preferably, the reduction temperature is 400°C, the reduction time is 2h), introduce the reaction gas in the temperature range of 50-400°C (preferably, the volume space velocity is 10000ml / (g*h)-50000ml / (g*h), more preferably, the volume space velocity is 20000ml / (g*h)-30000ml / (g*h)) to obtain the product.

9. The use according to claim 8, characterized in that: The reaction gas is a mixed gas containing 0.1-0.5% CO and 0.1-0.5% NO by volume (preferably, the volume concentration of CO and NO is 0.1-0.4%, more preferably, the volume concentration of CO and NO is 0.1-0.2%; preferably, the molar ratio of CO to NO is 1:1.2, more preferably, the molar ratio of CO to NO is 1:1), and the remaining components in the mixed gas are one or more of He gas and Ar gas.

Citation Information

Patent Citations

  • Supported Pd-based bimetallic nano-catalyst for reducing NO by CO

    CN114870865A

  • Supported monatomic synergistic nanoparticle bimetallic catalyst as well as preparation and application thereof

    CN115138359A

  • Alloyed metal catalysts for the reduction of NOx in the exhaust gases from internal combustion engines containing excess oxygen