Method for repairing imperfection of pseudo-classic architecture through 3D printing
Through the combination of 3D printing technology and special materials, the problem of incomplete repair effects and insufficient lifespan of antique buildings has been solved, and efficient and stable repair effects have been achieved, which is suitable for widespread promotion.
Patent Information
- Application Number
- CN202411104502.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-29
AI Technical Summary
The repair effect and service life of existing antique building repair methods are relatively insufficient, making it difficult to effectively solve the difficulties of repairing incomplete antique buildings.
Using 3D printing technology, a three-dimensional model is built by cleaning and scanning architectural defects, and special printing materials are used to print physical repairs, which are placed in slurry and cured, and the gaps are filled to complete the repair. The printing material is composed of photosensitive resin, functional additives, nanofiber materials, fly ash and deionized water, and is cured and aged using a slurry of polyamide epoxy resin and ferroferrite magnetic powder.
Efficient repair of incomplete antique buildings is achieved. The printed entity is stable and durable, repels insects, ensures service life, and improves the quality and quality of repairs.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building restoration, and in particular to a method for repairing defects of antique buildings using 3D printing. Background Art
[0002] Antique architectural forms can be divided into broad and narrow meanings. The broad sense of antique architectural forms refers to the use of modern or traditional building materials to re-create ancient architectural forms in line with traditional cultural characteristics; the narrow sense of antique architectural forms refers to the use of traditional building materials to restore ancient buildings within a specific range.
[0003] In the patent document with application number "CN202111186787.1" and titled "A method for repairing the wall of an antique building", it is recorded that "it includes the following steps: preparing cement mortar with cement, sand, and polyvinyl formal adhesive; mixing quicklime powder with water and aging to obtain lime milk; evenly mixing lime milk with straw stalks, fly ash, and cement mortar to obtain straw ash; evenly mixing lime milk with green alum water to obtain lime mortar; knocking and shoveling away all debris on the wall of the antique building to be repaired; applying the base layer with cement mortar; applying the transition coating with straw ash; and applying the topcoat with lime mortar. By adopting the technical solution of the present invention, by adding polyvinyl formal adhesive to the cement mortar, the adhesion of the cement mortar is increased, and the service life of the cement mortar is extended. By applying straw ash, the material components in the transition coating are tightly connected as one, which effectively prevents cracks in the wall. The color of the topcoat is adjusted by adding green alum water, thereby restoring the old appearance of the exterior wall of the antique building."
[0004] Although the method provided by the above patent document can repair antique buildings, its repair effect and service life are relatively insufficient and still need further improvement. Based on this, the present invention provides a method for repairing the defects of antique buildings by 3D printing to solve the above technical problems! Summary of the invention
[0005] The purpose of the present invention is to provide a method for repairing defects of antique buildings by 3D printing, which can perform three-dimensional modeling on all defects within the repair range, and can effectively solve the difficulties in repairing defects of antique buildings. The printed entity is not only stable and durable, but also insect-repellent, ensuring the service life. At the same time, the use of slurry effectively guarantees its quality.
[0006] To achieve the above object, the present invention provides the following technical solutions: The present invention provides a method for repairing defects of antique buildings by 3D printing, comprising the following steps: S1. Clean the dust and debris from the damaged parts of the antique buildings, use scanning equipment to scan the damaged parts of the ancient buildings, and build a three-dimensional model; S2, printing a physical repair object using a 3D printing device and printing materials according to the constructed three-dimensional model; S3, placing the printed solid repair object in slurry for treatment, and then placing it on the damaged part of the antique building for solidification, and filling the gap between the solid repair object and the damaged part of the antique building with slurry, and making it look old after solidification, thereby completing the repair of the damaged antique building.
[0007] The present invention is further configured as follows: in step S2, the printing material is composed of the following raw materials in parts by weight: 20 to 30 parts of photosensitive resin, 4 to 6 parts of functional additives, 2 to 5 parts of nanofiber materials, 1 to 4 parts of fly ash, 3 to 7 parts of polyethylene glycol and 30 to 40 parts of deionized water; The preparation process of the printing material is as follows: Accurately weigh photosensitive resin, functional additive, nanofiber material, fly ash, polyethylene glycol and deionized water, place the photosensitive resin, functional additive, polyethylene glycol and deionized water in a stirring device, and mix them at 120-220 r / min for 10-15 minutes; Then, the nanofiber material and fly ash are added, and mixed for 20 to 24 minutes at 80 to 100 r / min to obtain the printing material.
[0008] The present invention is further configured as follows: the preparation process of the functional additive is as follows: Soak an appropriate amount of the composite material in deionized water at a solid-liquid ratio of 0.12 to 0.52 g / mL for 20 to 30 minutes at room temperature, then heat it to 40 to 42°C and perform microwave treatment; After the microwave treatment is completed, the product is boiled and extracted for 50 to 60 minutes, cooled to room temperature, filtered, concentrated under reduced pressure, and dried to obtain a functional additive.
[0009] The present invention is further configured as follows: the composite material is formed by mixing camphor leaf powder and wormwood leaf powder in a mass ratio of 1:0.12-0.22.
[0010] The present invention is further configured as follows: the power of the microwave treatment is 480-500W, and the time is 20-30min.
[0011] The present invention is further configured as follows: the nanofiber material is formed by mixing nano glass fibers and nano carbon fibers in a mass ratio of 1:0.2 to 0.5.
[0012] The present invention is further configured as follows: in step S3, the printed physical repair object is immersed in the slurry for 5 to 10 seconds.
[0013] The present invention is further configured as follows: in step S3, the slurry is mixed with polyamide epoxy resin, ferroferric oxide magnetic powder, cement powder and water in a mass ratio of 1:0.11-0.22:0.4-0.6:5-7.
[0014] Compared with the prior art, the present invention has the following beneficial effects: The method for repairing the defects of antique buildings by 3D printing provided by the present invention is to clean the dust and debris at the defects of the antique buildings, use scanning equipment to scan the defects of the ancient buildings, and construct a three-dimensional model. According to the constructed three-dimensional model, the 3D printing equipment uses printing materials to print out a solid repair object, and the printed solid repair object is placed in a slurry for treatment, and then placed in the defect of the antique building for solidification, and the gap between the solid repair object and the defect of the antique building is filled in the slurry, and the antique building is aged after solidification to complete the repair of the defect of the antique building; the method of the present invention can perform three-dimensional modeling on all defects within the repair range, and can efficiently solve the difficulties in repairing the defects of antique buildings. The printed entity is not only stable and durable, but also repels insects, ensuring the service life. At the same time, the slurry is used to effectively ensure its quality. The method for repairing the defects of antique buildings by 3D printing provided by the present invention has a broader market prospect and is more suitable for promotion. DETAILED DESCRIPTION
[0015] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1
[0016] This embodiment provides a method for repairing defects of antique buildings by 3D printing, comprising the following steps: S1. Clean the dust and debris from the damaged parts of the antique buildings, use scanning equipment to scan the damaged parts of the ancient buildings, and build a three-dimensional model.
[0017] S2. Printing a solid repair object using printing materials using a 3D printing device according to the constructed three-dimensional model.
[0018] The printing material is composed of the following raw materials by weight: 20 parts of photosensitive resin, 4 parts of functional additives, 2 parts of nanofiber materials, 1 part of fly ash, 3 parts of polyethylene glycol and 30 parts of deionized water; In addition, the preparation process of printing materials is as follows: Accurately weigh photosensitive resin, functional additives, nanofiber material, fly ash, polyethylene glycol and deionized water, place the photosensitive resin, functional additives, polyethylene glycol and deionized water in a stirring device, and mix them at 120 r / min for 10 min; Then, nanofiber material and fly ash were added and mixed at 80 r / min for 20 min to obtain printing material.
[0019] Further, the preparation process of the functional additive is as follows: An appropriate amount of the composite material was placed in deionized water at a solid-liquid ratio of 0.12 g / mL and soaked for 20 min at room temperature, then heated to 40°C and then microwaved; After the microwave treatment, the product was boiled and extracted for 50 minutes, cooled to room temperature, filtered, concentrated under reduced pressure, and dried to obtain a functional additive.
[0020] Furthermore, the composite material is mixed by camphor leaf powder and mugwort leaf powder in a mass ratio of 1:0.12.
[0021] The power of microwave treatment was 480 W and the time was 20 min.
[0022] In addition, the nanofiber material is a mixture of nano glass fiber and nano carbon fiber in a mass ratio of 1:0.2.
[0023] In this embodiment, it should be noted that the photosensitive resin was purchased from Dongguan Jingshang New Material Development Co., Ltd., the fly ash was purchased from Hebei Zongrun Mineral Products Co., Ltd., the nano-glass fiber was purchased from Lianyungang Wohua New Material Technology Co., Ltd., and the nano-carbon fiber was purchased from Suzhou Beike Nano Technology Co., Ltd.
[0024] S3, placing the printed solid repair object in slurry for treatment, and then placing it on the damaged part of the antique building for solidification, and filling the gap between the solid repair object and the damaged part of the antique building with slurry, and making it look old after solidification, thereby completing the repair of the damaged antique building.
[0025] The printed solid repair object is immersed in the slurry for 5 seconds.
[0026] The slurry is prepared by mixing polyamide epoxy resin, ferroferric oxide magnetic powder, cement powder and water in a mass ratio of 1:0.11:0.4:5.
[0027] In this embodiment, it should be noted that the polyamide epoxy resin was purchased from Wuhan Jiyesheng Chemical Co., Ltd. Example 2
[0028] This embodiment provides a method for repairing defects of antique buildings by 3D printing, comprising the following steps: S1. Clean the dust and debris from the damaged parts of the antique buildings, use scanning equipment to scan the damaged parts of the ancient buildings, and build a three-dimensional model.
[0029] S2. Printing a solid repair object using printing materials using a 3D printing device according to the constructed three-dimensional model.
[0030] The printing material is composed of the following raw materials by weight: 22 parts of photosensitive resin, 5 parts of functional additives, 3 parts of nanofiber material, 2 parts of fly ash, 4 parts of polyethylene glycol and 32 parts of deionized water; In addition, the preparation process of printing materials is as follows: Accurately weigh photosensitive resin, functional additive, nanofiber material, fly ash, polyethylene glycol and deionized water, place the photosensitive resin, functional additive, polyethylene glycol and deionized water in a stirring device, and mix them at 122 r / min for 11 minutes; Then, nanofiber material and fly ash were added and mixed at 82 r / min for 22 min to obtain printing material.
[0031] Further, the preparation process of the functional additive is as follows: An appropriate amount of the composite material was placed in deionized water at a solid-liquid ratio of 0.14 g / mL and soaked for 22 min at room temperature, then heated to 41°C and subjected to microwave treatment; After the microwave treatment, the product was boiled and extracted for 52 minutes, cooled to room temperature, filtered, concentrated under reduced pressure, and dried to obtain a functional additive.
[0032] Furthermore, the composite material is mixed by camphor leaf powder and mugwort leaf powder in a mass ratio of 1:0.14.
[0033] The power of microwave treatment was 482 W and the time was 22 min.
[0034] In addition, the nanofiber material is a mixture of nano glass fiber and nano carbon fiber in a mass ratio of 1:0.3.
[0035] In this embodiment, it should be noted that the photosensitive resin was purchased from Dongguan Jingshang New Material Development Co., Ltd., the fly ash was purchased from Hebei Zongrun Mineral Products Co., Ltd., the nano-glass fiber was purchased from Lianyungang Wohua New Material Technology Co., Ltd., and the nano-carbon fiber was purchased from Suzhou Beike Nano Technology Co., Ltd.
[0036] S3, placing the printed solid repair object in slurry for treatment, and then placing it on the damaged part of the antique building for solidification, and filling the gap between the solid repair object and the damaged part of the antique building with slurry, and making it look old after solidification, thereby completing the repair of the damaged antique building.
[0037] The printed solid repair object is immersed in the slurry for 6 seconds.
[0038] The slurry is prepared by mixing polyamide epoxy resin, ferroferric oxide magnetic powder, cement powder and water in a mass ratio of 1:0.13:0.5:6.
[0039] In this embodiment, it should be noted that the polyamide epoxy resin was purchased from Wuhan Jiyesheng Chemical Co., Ltd. Example 3
[0040] This embodiment provides a method for repairing defects of antique buildings by 3D printing, comprising the following steps: S1. Clean the dust and debris from the damaged parts of the antique buildings, use scanning equipment to scan the damaged parts of the ancient buildings, and build a three-dimensional model.
[0041] S2. Printing a solid repair object using printing materials using a 3D printing device according to the constructed three-dimensional model.
[0042] The printing material is composed of the following raw materials by weight: 25 parts of photosensitive resin, 5 parts of functional additives, 3 parts of nanofiber material, 2 parts of fly ash, 5 parts of polyethylene glycol and 35 parts of deionized water; In addition, the preparation process of printing materials is as follows: Accurately weigh photosensitive resin, functional additives, nanofiber material, fly ash, polyethylene glycol and deionized water, place the photosensitive resin, functional additives, polyethylene glycol and deionized water in a stirring device, and mix them at 170 r / min for 12 minutes; Then, nanofiber material and fly ash were added and mixed at 90 r / min for 22 min to obtain printing material.
[0043] Further, the preparation process of the functional additive is as follows: An appropriate amount of the composite material was placed in deionized water at a solid-liquid ratio of 0.32 g / mL and soaked for 25 min at room temperature, then heated to 41°C and subjected to microwave treatment; After the microwave treatment, the product was boiled and extracted for 55 minutes, cooled to room temperature, filtered, concentrated under reduced pressure, and dried to obtain a functional additive.
[0044] Furthermore, the composite material is mixed by camphor leaf powder and wormwood leaf powder in a mass ratio of 1:0.17.
[0045] The power of microwave treatment was 490 W and the time was 25 min.
[0046] In addition, the nanofiber material is a mixture of nano glass fiber and nano carbon fiber in a mass ratio of 1:0.3.
[0047] In this embodiment, it should be noted that the photosensitive resin was purchased from Dongguan Jingshang New Material Development Co., Ltd., the fly ash was purchased from Hebei Zongrun Mineral Products Co., Ltd., the nano-glass fiber was purchased from Lianyungang Wohua New Material Technology Co., Ltd., and the nano-carbon fiber was purchased from Suzhou Beike Nano Technology Co., Ltd.
[0048] S3, placing the printed solid repair object in slurry for treatment, and then placing it on the damaged part of the antique building for solidification, and filling the gap between the solid repair object and the damaged part of the antique building with slurry, and making it look old after solidification, thereby completing the repair of the damaged antique building.
[0049] The printed solid repair object is immersed in the slurry for 7 seconds.
[0050] The slurry is prepared by mixing polyamide epoxy resin, ferroferric oxide magnetic powder, cement powder and water in a mass ratio of 1:0.17:0.5:6.
[0051] In this embodiment, it should be noted that the polyamide epoxy resin was purchased from Wuhan Jiyesheng Chemical Co., Ltd. Example 4
[0052] This embodiment provides a method for repairing defects of antique buildings by 3D printing, comprising the following steps: S1. Clean the dust and debris from the damaged parts of the antique buildings, use scanning equipment to scan the damaged parts of the ancient buildings, and build a three-dimensional model.
[0053] S2. Printing a solid repair object using printing materials using a 3D printing device according to the constructed three-dimensional model.
[0054] The printing material is composed of the following raw materials by weight: 28 parts of photosensitive resin, 5 parts of functional additives, 4 parts of nanofiber material, 3 parts of fly ash, 6 parts of polyethylene glycol and 38 parts of deionized water; In addition, the preparation process of printing materials is as follows: Accurately weigh photosensitive resin, functional additive, nanofiber material, fly ash, polyethylene glycol and deionized water, place the photosensitive resin, functional additive, polyethylene glycol and deionized water in a stirring device, and mix them at 210 r / min for 14 minutes; Then, nanofiber material and fly ash were added and mixed at 95 r / min for 23 min to obtain printing material.
[0055] Further, the preparation process of the functional additive is as follows: An appropriate amount of the composite material was placed in deionized water at a solid-liquid ratio of 0.42 g / mL and soaked for 28 min at room temperature, then heated to 41°C and subjected to microwave treatment; After the microwave treatment, the product was boiled and extracted for 58 minutes, cooled to room temperature, filtered, concentrated under reduced pressure, and dried to obtain a functional additive.
[0056] Furthermore, the composite material is mixed by camphor leaf powder and mugwort leaf powder in a mass ratio of 1:0.2.
[0057] The power of microwave treatment was 495 W and the time was 28 min.
[0058] In addition, the nanofiber material is a mixture of nano glass fiber and nano carbon fiber in a mass ratio of 1:0.4.
[0059] In this embodiment, it should be noted that the photosensitive resin was purchased from Dongguan Jingshang New Material Development Co., Ltd., the fly ash was purchased from Hebei Zongrun Mineral Products Co., Ltd., the nano-glass fiber was purchased from Lianyungang Wohua New Material Technology Co., Ltd., and the nano-carbon fiber was purchased from Suzhou Beike Nano Technology Co., Ltd.
[0060] S3, placing the printed solid repair object in slurry for treatment, and then placing it on the damaged part of the antique building for solidification, and filling the gap between the solid repair object and the damaged part of the antique building with slurry, and making it look old after solidification, thereby completing the repair of the damaged antique building.
[0061] The printed solid repair object was immersed in the slurry for 9 seconds.
[0062] The slurry is prepared by mixing polyamide epoxy resin, ferroferric oxide magnetic powder, cement powder and water in a mass ratio of 1:0.2:0.5:6.
[0063] In this embodiment, it should be noted that the polyamide epoxy resin was purchased from Wuhan Jiyesheng Chemical Co., Ltd. Example 5
[0064] This embodiment provides a method for repairing defects of antique buildings by 3D printing, comprising the following steps: S1. Clean the dust and debris from the damaged parts of the antique buildings, use scanning equipment to scan the damaged parts of the ancient buildings, and build a three-dimensional model.
[0065] S2. Printing a solid repair object using printing materials using a 3D printing device according to the constructed three-dimensional model.
[0066] The printing material is composed of the following raw materials by weight: 30 parts of photosensitive resin, 6 parts of functional additives, 5 parts of nanofiber material, 4 parts of fly ash, 7 parts of polyethylene glycol and 40 parts of deionized water; In addition, the preparation process of printing materials is as follows: Accurately weigh photosensitive resin, functional additives, nanofiber material, fly ash, polyethylene glycol and deionized water, place the photosensitive resin, functional additives, polyethylene glycol and deionized water in a stirring device, and mix them at 220 r / min for 15 minutes; Then, nanofiber material and fly ash were added and mixed at 100 r / min for 24 min to obtain printing material.
[0067] Further, the preparation process of the functional additive is as follows: An appropriate amount of the composite material was placed in deionized water at a solid-liquid ratio of 0.52 g / mL and soaked for 30 min at room temperature, then heated to 42°C and subjected to microwave treatment; After the microwave treatment, the product was boiled and extracted for 60 minutes, cooled to room temperature, filtered, concentrated under reduced pressure, and dried to obtain a functional additive.
[0068] Furthermore, the composite material is mixed by camphor leaf powder and mugwort leaf powder in a mass ratio of 1:0.22.
[0069] The power of microwave treatment was 500 W and the time was 30 min.
[0070] In addition, the nanofiber material is a mixture of nano glass fiber and nano carbon fiber in a mass ratio of 1:0.5.
[0071] In this embodiment, it should be noted that the photosensitive resin was purchased from Dongguan Jingshang New Material Development Co., Ltd., the fly ash was purchased from Hebei Zongrun Mineral Products Co., Ltd., the nano-glass fiber was purchased from Lianyungang Wohua New Material Technology Co., Ltd., and the nano-carbon fiber was purchased from Suzhou Beike Nano Technology Co., Ltd.
[0072] S3, placing the printed solid repair object in slurry for treatment, and then placing it on the damaged part of the antique building for solidification, and filling the gap between the solid repair object and the damaged part of the antique building with slurry, and making it look old after solidification, thereby completing the repair of the damaged antique building.
[0073] The printed solid repair object is immersed in the slurry for 10 seconds.
[0074] The slurry is prepared by mixing polyamide epoxy resin, ferroferric oxide magnetic powder, cement powder and water in a mass ratio of 1:0.22:0.6:7.
[0075] In this embodiment, it should be noted that the polyamide epoxy resin was purchased from Wuhan Jiyesheng Chemical Co., Ltd.
[0076] The 3D printing method for repairing antique building defects provided by the present invention can perform three-dimensional modeling of all defects within the repair range, and can effectively solve the difficulties in repairing antique building defects. The printed entity is not only stable and durable, but also repels insects, ensuring the service life. At the same time, the slurry is used to effectively ensure its quality. This shows that the 3D printing method for repairing antique building defects provided by the present invention has a broader market prospect and is more suitable for promotion.
[0077] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0078] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for repairing defects in antique buildings by 3D printing, characterized in that: The following steps are involved: S1. Clean the dust and debris from the damaged parts of the antique buildings, use scanning equipment to scan the damaged parts of the ancient buildings, and build a three-dimensional model; S2, printing a physical repair object using a 3D printing device and printing materials according to the constructed three-dimensional model; S3, placing the printed solid repair object in slurry for treatment, and then placing it on the damaged part of the antique building for solidification, and filling the gap between the solid repair object and the damaged part of the antique building with slurry, and making it look old after solidification, thereby completing the repair of the damaged antique building.
2. The method for repairing defects of antique buildings by 3D printing according to claim 1, characterized in that: In step S2, the printing material is composed of the following raw materials in parts by weight: 20 to 30 parts of photosensitive resin, 4 to 6 parts of functional additives, 2 to 5 parts of nanofiber material, 1 to 4 parts of fly ash, 3 to 7 parts of polyethylene glycol and 30 to 40 parts of deionized water; The preparation process of the printing material is as follows: Accurately weigh photosensitive resin, functional additive, nanofiber material, fly ash, polyethylene glycol and deionized water, place the photosensitive resin, functional additive, polyethylene glycol and deionized water in a stirring device, and mix them at 120-220 r / min for 10-15 minutes; Then, the nanofiber material and fly ash are added, and mixed for 20 to 24 minutes at 80 to 100 r / min to obtain the printing material.
3. The method for repairing defects of antique buildings by 3D printing according to claim 2, characterized in that: The preparation process of the functional additive is as follows: Soak an appropriate amount of the composite material in deionized water at a solid-liquid ratio of 0.12 to 0.52 g / mL for 20 to 30 minutes at room temperature, then heat it to 40 to 42°C and perform microwave treatment; After the microwave treatment is completed, the product is boiled and extracted for 50 to 60 minutes, cooled to room temperature, filtered, concentrated under reduced pressure, and dried to obtain a functional additive.
4. The method for repairing defects of antique buildings by 3D printing according to claim 3, characterized in that: The composite material is prepared by mixing camphor leaf powder and wormwood leaf powder in a mass ratio of 1:0.12-0.
22.
5. The method for repairing defects of antique buildings by 3D printing according to claim 3, characterized in that: The power of the microwave treatment is 480-500W, and the time is 20-30min.
6. The method for repairing defects of antique buildings by 3D printing according to claim 2, characterized in that: The nanofiber material is formed by mixing nano glass fiber and nano carbon fiber in a mass ratio of 1:0.2-0.
5.
7. The method for repairing defects of antique buildings by 3D printing according to claim 1, characterized in that: In the step S3, the printed physical repair object is immersed in the slurry for 5 to 10 seconds.
8. The method for repairing defects of antique buildings by 3D printing according to claim 1, characterized in that: In step S3, the slurry is prepared by mixing polyamide epoxy resin, ferroferric oxide magnetic powder, cement powder and water in a mass ratio of 1:0.11-0.22:0.4-0.6:5-7.
Citation Information
Patent Citations
Historic building carving decoration repairing method based on 3D technology
CN103264605A
Mosquito and insect repelling concrete
CN105130323A
Biological high-fidelity restoration method for damaged part of stone cultural relic based on 3D printing
CN115536315A
Method for repairing ancient building crack by using 3D printing model
CN116290880A
Method for carrying out magnetization plugging by using oily epoxy resin magnetic slurry