Porous carbon material as well as preparation method and application thereof
Through the blending reaction and carbonization method of small organic amine molecules with amine activators and acids, the problems of equipment corrosion and environmental pollution in the preparation of porous carbon materials are solved, and the preparation of porous carbon materials with high specific surface area is realized, and the process flow is simplified. And improve yield and morphological control.
Patent Information
- Application Number
- CN202310497016.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-05
- Publication Date
- 2024-11-05
AI Technical Summary
The existing methods for preparing porous carbon materials have problems such as serious equipment corrosion, serious environmental pollution, low product recovery rate, high activation temperature, long activation time, high template cost and cumbersome template removal.
Using small organic amine molecules to blend with amine activators and acids to obtain a precursor, and then carbonize in an inert atmosphere, adjust the reaction conditions to prepare porous carbon materials with high specific surface area, avoiding equipment corrosion and environment in traditional methods Pollution simplifies the process flow.
The preparation of porous carbon materials with a high specific surface area is achieved, with simple process, environmentally friendly, corrosion-free equipment, controllable product morphology and size, high yield, short activation time, and no need for pickling to remove alkali metals.
Smart Images

Figure CN118894514A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of energy storage such as supercapacitors and lead-acid batteries, and specifically relates to a porous carbon material and a preparation method and use thereof, and also specifically relates to a porous carbon material prepared from organic amine molecules and a preparation method and use thereof. Background Art
[0002] There are many methods for preparing porous carbon materials, mainly including: chemical activation method, physical activation method, template method, self-activation method, polymer direct thermal decomposition method, etc. (DOI: 10.1002 / smtd.201900853). Among them, KOH chemical activation is the most common method for preparing porous carbon (DOI: 10.1007 / s40242-018-8127-9). Its main problem is that KOH seriously corrodes the activation equipment; physical activation mainly uses water vapor or carbon dioxide to activate the carbon source at a high temperature above 900°C. The main problems of this method are high activation temperature, long activation time and low product recovery rate; template method is a common method for preparing porous carbon materials with specific pore sizes, but this method has the problems of high cost of the template itself and cumbersome template removal (DOI: 10.1002 / aenm.201100654); self-activation method uses some organic alkali metal salts (such as potassium acetate, lemon) to activate the carbon source. The method requires specific organic matter and needs to be acid-washed after activation to remove the alkali metal element and alkali metal carbonate generated during the activation process (DOI: 10.1016 / j.carbon.2021.06.072); the direct pyrolysis of polymers is a controllable, simple method without activator residues, but the precursor preparation of this method is complicated and the monomers used are expensive (DOI: 10.1021 / acs.chemmater.9b02918; DOI: 10.1038 / ncomms8221); some researchers used methanol as solvent, reacted p-phenylenediamine with sulfuric acid, and then evaporated the methanol to obtain pDA [H 2 SO 4 ], adding ammonium persulfate aqueous solution, then reacting at 80°C for 24h, washing with ethanol, and directly carbonizing after drying to obtain porous carbon (DOI:10.1016 / j.cej.2017.02.110), but the porous carbon synthesized by this method has a small specific surface area and poor capacitance performance. Summary of the invention
[0003] In order to improve the above technical problems, the present invention provides a porous carbon material prepared by organic amine molecules, and a preparation method and application thereof, which can solve the problems of severe equipment corrosion, severe environmental pollution, low product recovery rate and complex process in the chemical activation method; low product yield, high activation temperature and long activation time in the physical activation method; and high cost of the template itself and cumbersome template removal in the template method.
[0004] The technical solution of the present invention is as follows:
[0005] A method for preparing a porous carbon material using small organic amine molecules, the method comprising the following steps:
[0006] (1) mixing an organic amine small molecule, an amine activator, and an acid to react to obtain a precursor;
[0007] (2) Carbonization: heating and carbonizing the precursor to prepare the porous carbon material.
[0008] According to an embodiment of the present invention, in step (1), the organic amine small molecule is selected from one or more mixed organic amines of amines that can initiate polymerization, such as aniline, m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, naphthylamine, pyrrole, diaminonaphthalene, m-phenylenediamine, diaminoanthraquinone, diphenylamine, dinaphthylamine, diaminopyrrole, caprolactam, etc.
[0009] According to an embodiment of the present invention, in step (1), the amine activator is selected from a mixture of one or more of urea, melamine, cyanamide, ethylenediamine, thiourea, dicyandiamide, etc.
[0010] According to an embodiment of the present invention, in step (1), the acid comprises: one or more mixed acids selected from boric acid, citric acid, phosphoric acid, phytic acid, sulfuric acid, hydrochloric acid, nitric acid, cyanuric acid, ethylenediaminetetraacetic acid, etc. The acid is in the form of an acid solution, such as an acid aqueous solution; the concentration of the acid solution is, for example, 0.1-18.4 mol / L, preferably 1-5 mol / L.
[0011] According to an embodiment of the present invention, in step (1), the organic amine small molecule and the amine activator are first mixed, and then an acid is added for reaction.
[0012] According to an embodiment of the present invention, in step (1), the reaction temperature is 0°C to 300°C, preferably 30-120°C, and the reaction time is not less than 1 hour, for example 1-48 hours, preferably 2-24 hours.
[0013] According to an embodiment of the present invention, in step (1), the mass volume ratio of the organic amine small molecule and the amine activator and the acid is 10 (g): 0.05-20 (g): 20-80 (mL), preferably 10 (g): 1-10 (g): 20-60 (mL).
[0014] According to an embodiment of the present invention, step (1) further comprises a post-treatment step of filtering and drying the prepared product to obtain a precursor.
[0015] According to an embodiment of the present invention, in step (2), the carbonization is carried out under an inert gas, and the inert gas is selected from one or more of nitrogen, argon, hydrogen, helium, etc.
[0016] According to an embodiment of the present invention, in step (2), the carbonization temperature is 400°C to 1000°C, and is exemplarily 500°C, 600°C, 700°C, 800°C, 900°C, and 1000°C. The carbonization time is 0.5-24h, preferably 0.5-12h, and is exemplarily 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, and 12h. That is, the carbonization refers to directly heating from 0°C to 500-1000°C for carbonization.
[0017] According to an embodiment of the present invention, in step (2), the carbonization includes two steps: first, pre-carbonization at 400-700°C for 0.5-6h, and then heating to 750-1000°C for high-temperature carbonization for 0.5-6h.
[0018] According to an embodiment of the present invention, in step (2), before carbonization, the precursor may be reacted with an oxidant, and / or polymerized under an oxygen atmosphere to prepare a mixture.
[0019] According to an embodiment of the present invention, the oxidant is selected from at least one of ammonium persulfate, ferric chloride, hydrogen peroxide, potassium permanganate, potassium ferrate and the like.
[0020] According to an embodiment of the present invention, the oxygen atmosphere refers to an atmosphere containing oxygen. The polymerization reaction is carried out in an oxygen atmosphere at a temperature of 100°C to 400°C, exemplarily 100°C, 200°C, 300°C, and 400°C.
[0021] According to an embodiment of the present invention, the specific surface area of the porous carbon is at least 1000 m 2 / g, preferably 1500-2000m 2 In the present invention, the specific surface area can be adjusted by adjusting the feed ratio of each raw material.
[0022] As an exemplary embodiment of the present invention, the method for preparing porous carbon materials with small organic amine molecules specifically includes:
[0023] Step 1: Precursor preparation:
[0024] An organic amine (such as one or more mixed organic amines of amines that can initiate polymerization, such as aniline, m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, naphthylamine, pyrrole, diaminonaphthalene, m-phenylenediamine, diaminoanthraquinone, benzidine, dinaphthylamine, diaminopyrrole, caprolactam, etc.) and an amine activator (such as one or more mixed amines of urea, melamine, aminocyanide, ethylenediamine, thiourea, dicyandiamide, etc.), and then one or more acids (such as boric acid, citric acid, phosphoric acid, phytic acid, sulfuric acid, hydrochloric acid, nitric acid, cyanuric acid, ethylenediaminetetraacetic acid, etc.) are added to react at 0°C to 300°C for at least 1h to obtain a precursor;
[0025] Step 2 Carbonization:
[0026] Carbonizing the precursor at 500° C. to 1000° C. in an inert atmosphere (e.g., one or any mixed gas of nitrogen, argon, hydrogen, helium, etc.) to obtain a porous carbon material;
[0027] Alternatively, S1: when preparing a precursor, an oxidant (for example, one or more of ammonium persulfate, ferric chloride, hydrogen peroxide, potassium permanganate, potassium ferrate, etc.) is added and mixed for polymerization; the polymerization product is carbonized under an inert atmosphere (for example, one or more of nitrogen, argon, hydrogen, helium, etc.) at 400° C. to 1000° C. to obtain a porous carbon material;
[0028] Alternatively, S2: polymerize the precursor in an oxidizing atmosphere (e.g., an atmosphere containing oxygen) at 100°C to 400°C; carbonize the polymerization product in an inert atmosphere (e.g., one or any mixed gas of nitrogen, argon, hydrogen, helium, etc.) at 400°C to 1000°C to obtain a porous carbon material.
[0029] The invention also provides a porous carbon material prepared by the method.
[0030] The present invention also provides an application of the porous carbon material in energy storage fields such as supercapacitors and lead-acid batteries.
[0031] Beneficial effects of the present invention:
[0032] The present invention provides a method for preparing porous carbon materials from organic amine small molecules. The method utilizes the different physical and chemical properties of organic amine small molecules to mix a variety of organic amine small molecules with an acid to undergo a Lewis acid-base reaction to obtain a precursor, and then obtain the porous carbon material through polymerization-carbonization; or directly carbonize the carbon precursor to obtain the porous carbon material. Compared with the traditional alkali activation method, physical activation method, and hard template method, the method of the present invention has simple process, low environmental pollution, no corrosion to equipment, controllable product morphology and size, high specific surface area, high yield, short activation time, and no need for acid washing. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The SEM image (a) and capacitance performance (b) of the porous carbon material prepared in Example 1;
[0034] Figure 2 The SEM image (a) and capacitance performance (b) of the porous carbon material prepared in Example 2;
[0035] Figure 3 are precursors of different morphologies prepared in Example 3;
[0036] Figure 4 These are the SEM photograph (a) and capacitance performance (b) of the porous carbon material prepared in Comparative Example 1. DETAILED DESCRIPTION
[0037] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0038] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0039] Example 1
[0040] Step 1: Weigh 10g p-phenylenediamine and 1g melamine and add them into 50mL 1mol / L H 2 SO 4 The precursor was obtained by stirring the reaction at 80°C for 6 h in aqueous solution, filtering, and drying with forced air at 60°C for 12 h.
[0041] Step 2: polymerize the precursor at 200 °C for 6 h in an oxygen atmosphere;
[0042] Step 3: The sample after oxygen polymerization was pre-carbonized at 550℃ for 6h in a nitrogen atmosphere, and then heated to 800℃ for carbonization for 2h to obtain a specific surface area of 1581m 2 / g of porous carbon material. The SEM and capacitance properties of the obtained porous carbon material are shown in Figure 1 shown.
[0043] Example 2
[0044] Step 1: Weigh 10g p-phenylenediamine and 3g urea and add them to 50mL 1mol / L H 2 SO 4 The reaction was stirred in aqueous solution at room temperature for 6 h, filtered, and dried at 60 °C for 12 h to obtain the precursor;
[0045] Step 2: The precursor was pre-carbonized at 600 °C for 3 h in a nitrogen atmosphere, and then heated to 800 °C for carbonization for 2 h to obtain a specific surface area of 1697 m 2 / g of porous carbon material. The SEM and capacitance properties of the obtained porous carbon material are shown in Figure 2 Shown
[0046] Example 3
[0047] Weigh 10g p-phenylenediamine and 3g urea, p-phenylenediamine: sulfuric acid (H 2 SO 4 The molar ratios of the reaction mixture (concentration of 1 mol / L) were 1:0.5 and 1:1, respectively. The reaction was stirred at room temperature for 6 h, filtered, and dried at 60 °C for 12 h to obtain precursors with different morphologies. The SEM images of the obtained precursors are shown in Figure 3 As shown. Among them, Figure 3 a is a molar ratio of 1:1, Figure 3 b is a molar ratio of 1:0.5;
[0048] The remaining steps are the same as those in Example 1.
[0049] Comparative Example 1
[0050] Step 1: Weigh 10g of p-phenylenediamine and add it to 50mL of 1mol / L H 2 SO 4 The reaction was stirred in aqueous solution at room temperature for 6 h, filtered, and dried at 60 °C for 12 h to obtain the precursor;
[0051] Step 2: Carbonize the precursor in a nitrogen atmosphere at 800 °C for 0.5 h to obtain a specific surface area of 1100 m 2 / g of porous carbon material. The SEM and capacitance properties of the obtained porous carbon material are shown in Figure 4 shown.
[0052] Test Example 1
[0053] Capacitor performance test
[0054] Take 40 mg of the porous carbon material prepared in the above Examples 1-2 and Comparative Example 1, 9.5 mL of isopropanol solution (the volume ratio of isopropanol to water is 3:1), and 0.5 mL of Nafion solution, and ultrasonically disperse. Drop the dispersed slurry onto a glassy carbon rod with a diameter of 5 mm. After the electrode is dried, use a three-electrode system using a Chenhua CHI760e electrochemical workstation, with a platinum wire electrode as the counter electrode, a saturated silver chloride electrode as the reference electrode, and 5 mol / L sulfuric acid as the electrolyte. The test results are as follows Figure 1 From the results of 1b, 2b and 4b, it can be seen that the addition of amine activators can change the pore structure of porous carbon, thereby improving the electrochemical performance; and different amine activators have different effects.
[0055] The above is an exemplary description of the embodiments of the present invention. However, the protection scope of the present invention is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing porous carbon materials using small organic amine molecules, characterized in that: The method comprises the following steps: (1) mixing an organic amine small molecule, an amine activator, and an acid to obtain a precursor; (2) Carbonization: heating and carbonizing the precursor to prepare the porous carbon material.
2. The method according to claim 1, characterized in that In step (1), the organic amine small molecule is selected from one or more mixed organic amines of amines that can initiate polymerization, such as aniline, m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, naphthylamine, pyrrole, diaminonaphthalene, m-phenylenediamine, diaminoanthraquinone, benzidine, dinaphthylamine, diaminopyrrole, caprolactam, etc. Preferably, in step (1), the amine activator is selected from a mixture of one or more of urea, melamine, cyanamide, ethylenediamine, thiourea and dicyandiamide.
3. The method according to claim 1 or 2, characterized in that: In step (1), the acid comprises: one or more mixed acids selected from the group consisting of boric acid, citric acid, phosphoric acid, phytic acid, sulfuric acid, hydrochloric acid, nitric acid, cyanuric acid, and ethylenediaminetetraacetic acid.
4. The method according to any one of claims 1 to 3, characterized in that: In step (1), the reaction temperature is 0°C to 300°C, and the reaction time is not less than 1 hour. Preferably, in step (1), the mass volume ratio of the organic amine small molecule to the amine activator and the acid is 10 (g): 0.05-20 (g): 20-80 (mL).
5. The method according to any one of claims 1 to 4, characterized in that: In step (2), the carbonization is carried out under an inert gas, and the inert gas is selected from one or more of nitrogen, argon, hydrogen and helium.
6. The method according to any one of claims 1 to 5, characterized in that: In step (2), the carbonization temperature is 400° C. to 1000° C., and the carbonization time is 0.5 to 24 hours; Alternatively, in step (2), the carbonization includes two steps: pre-carbonization at 400-700°C for 0.5-6h, and then high-temperature carbonization at 750-1000°C for 0.5-6h.
7. The method according to any one of claims 1 to 6, characterized in that: In step (2), before carbonization, the precursor may be reacted with an oxidant and / or polymerized in an oxygen atmosphere to prepare a mixture. Preferably, the oxidant is selected from at least one of ammonium persulfate, ferric chloride, hydrogen peroxide, potassium permanganate and potassium ferrate. Preferably, the oxygen atmosphere refers to an atmosphere containing oxygen. The polymerization reaction temperature in the oxygen atmosphere is 100° C. to 400° C.
8. The method according to any one of claims 1 to 7, characterized in that: The specific surface area of the porous carbon is at least 1000 m 2 / g.
9. The porous carbon material prepared by the method according to any one of claims 1 to 8.
10. Application of the porous carbon material according to claim 9 in the field of supercapacitor and lead-acid battery energy storage.
Citation Information
Cited By
Biomass-based porous carbon material as well as preparation method and application thereof
CN121948427A