Hypoeutectoid turnout rail in high-cold region and heat treatment production method

By adopting specific component design and multi-section heat treatment technology in railway switch rails in high-altitude areas, sub-eutectoid switch rails in high-altitude areas are formed, which solves the wear and fatigue problems of switches in complex environments, and significantly improves its strength and corrosion resistance. Meet the high-performance needs of railways in high-altitude areas.

CN118895407APending Publication Date: 2024-11-05PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP

Patent Information

Application Number
CN202411097828.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Railway switches in high-altitude areas are prone to severe wear, fatigue and heat damage in complex environments. The existing U71Mn hot-rolled rails or heat-treated rails have shortcomings in wear resistance, fatigue resistance and corrosion resistance, which cannot meet the high strength and toughness of railways in high-altitude areas. and corrosion resistance requirements.

Method used

The smelting cast steel billet is designed using components of 0.50%-0.70% carbon, 0.25%≤Cr+V≤0.50%, 2.5%≤Cu or Ni≤3.5%, and the subeutectomy switch rails in the high-altitude area are formed by step-by-step cooling through multi-stage heat treatment. The rolling waste heat is heat treated online, and the final cooling temperature and cooling rate are controlled to improve the phase change supercooling degree and tissue refinement to form pearlite + a small amount of ferrite tissue.

Benefits of technology

Improve the tensile strength, elongation, surface hardness and wear resistance of the switch rail, enhance corrosion resistance, and improve corrosion resistance by more than 30% and wear resistance by more than 35% compared with the existing U71Mn hot-rolled rail, suitable for high cold District railway.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895407A_ABST
    Figure CN118895407A_ABST
Patent Text Reader

Abstract

The invention discloses a hypoeutectoid turnout rail in an alpine region and a heat treatment production method. The method comprises the following steps: heating and rolling 0.50-0.70% C and smelted and cast steel billets into the turnout rail; rolling waste heat is utilized, an online heat treatment device is adopted, and cooling is conducted to the final cooling temperature in a multi-section heat treatment step-by-step cooling mode; cooling to room temperature at a first preset rate; and straightening and processing to obtain the hypoeutectoid turnout rail in the high-cold region. According to the invention, a hypoeutectoid structure is mainly obtained, and excellent toughness and plasticity are taken into account while the strength and hardness are ensured; cr + V is greater than or equal to 0.25% and less than or equal to 0.50%, so that a good grain and lamellar spacing refining effect is ensured, the obdurability is improved, and the hardness and wear resistance of the turnout rail are improved; rolling waste heat is utilized, based on the temperature change condition of the turnout rail in the cooling process, a large cooling speed is adopted before phase change, a slow cooling speed is adopted in the phase change process, and a rapid cooling speed is adopted after phase change. The phase change supercooling degree is improved, and meanwhile it is guaranteed that the structure is a pearlite and a small amount of ferritic structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of railway steel production, and in particular to a hypoeutectoid turnout rail for high-cold regions and a heat treatment production method. Background Art

[0002] Railways in high-cold areas are characterized by complex service environments and topography such as low temperature, humidity, wind, rain, snow, and fragile ecological areas. They will face more complex and changeable operating environment conditions. Turnouts are important components for guiding trains to turn. Turnout rails are important components for turnout manufacturing. The performance of turnout rails is directly related to the safety of railway train transportation and driving efficiency. Therefore, turnouts play a critical role in railways in high-cold areas.

[0003] As one of the most core and key components of the wheel-rail system, the turnout supports, guides and tractions the train through rolling contact between the wheel and rail, and its service behavior is directly related to the safety of train operation. As an open system, the turnout is in an open environment for a long time. When operating under the above-mentioned complex environment and long and steep slope line conditions, the track turnout and train wheels are very likely to suffer from severe wear, fatigue and thermal damage; in addition, the turnout must meet the high reliability operation under long-term high traction / braking force loads and frequent environmental changes, earthquakes and other emergency conditions, which will put forward extremely high requirements and new challenges for the safe and reliable service of the wheel-rail system. As the line with the most complex operating environment and working conditions, the Sichuan High-altitude Cold Area Railway faces the dual test of long and steep slopes and complex service environment. During the service process, a series of problems are very likely to occur, such as turnout tissue deterioration (plastic deformation and white layer formation), abrasions, thermal damage failure and fatigue failure, and wheel-rail interface adhesion.

[0004] The special lines and climatic conditions of the railway in the high-cold area have put forward high requirements on the contact fatigue resistance and toughness and plasticity of the turnout. The turnout is required to have a long service life. Conventional U71Mn hot-rolled rails or U71Mn heat-treated rails have deficiencies in wear resistance, fatigue resistance and corrosion resistance. Therefore, in view of the special requirements of the railway in the high-cold area for the performance of the turnout rail, an alternative new alloy system hypoeutectoid turnout rail with high strength and toughness, good rolling contact fatigue resistance and excellent corrosion resistance is urgently needed.

[0005] Based on this, the existing technology still needs to be improved. Summary of the invention

[0006] In order to solve the above technical problems, the embodiments of the present invention provide a hypoeutectoid turnout rail for high-cold areas and a heat treatment production method.

[0007] In order to solve the above technical problems, on the one hand, some embodiments of the present invention disclose a heat treatment production method for hypoeutectoid turnout rails in high-cold areas, comprising: The steel billet after smelting and casting is heated and rolled into a turnout rail; Utilizing the residual heat from rolling, an online heat treatment device is used to cool the steel to the final cooling temperature in a multi-stage heat treatment and step-by-step cooling manner; then cooling to room temperature at a first predetermined rate; After straightening and processing, it is made into hypoeutectoid turnout rail for high-altitude and cold regions.

[0008] In some embodiments, the smelting and casting adopts a composition design of 0.50%-0.70% carbon, 0.25%≤Cr+V≤0.50%, 2.5%≤Cu or Ni≤3.5%, based on weight percentage.

[0009] In some embodiments, the final rolling temperature of the steel billet during hot rolling is 850°C-950°C.

[0010] In some embodiments, the starting temperature of the step-by-step cooling in the multi-stage heat treatment is 740°C-850°C.

[0011] In some embodiments, the multi-stage heat treatment and step-by-step cooling include: The heat treatment was performed in 13 stages with a step-by-step cooling method. Stages 1-3 were cooled at 3.0°C / s -3.5°C / s, stages 4-6 were cooled at 2.5°C / s -3.0°C / s, stages 7-9 were cooled at 2.0°C / s -2.5°C / s, and stages 10-13 were cooled at 1.5°C / s -2.0°C / s.

[0012] In some embodiments, the final cooling temperature of the multi-stage heat treatment step-by-step cooling is 450°C-550°C.

[0013] In some embodiments, the alloy composition of the smelting and casting further includes, by weight percentage: 1.20%≤Si+Mn+P+S≤1.35%; Alternatively, the S content of the finished turnout rail is ≤0.008%, and the smelting process adopts 0.002%-0.010% low sulfur control.

[0014] On the other hand, an embodiment of the present invention further discloses a hypoeutectoid turnout rail for high-cold regions, which is manufactured by the aforementioned heat treatment production method for hypoeutectoid turnout rail for high-cold regions.

[0015] In some embodiments, the tensile strength is 1105-1212 MPa, the elongation is 12%-18%, the surface hardness is 320-360 HB; and the residual stress at the rail bottom is ≤250 MPa.

[0016] In some embodiments, 0.01 mol / L NaHSO 3 The solution is a corrosive solution, the corrosion time is 40 days, and the corrosion weight gain is 9 mg / cm 2 -17mg / cm 2 ; Alternatively, with a loading force of 980N, after 100,000 cycles, the wear amount is 0.26g-0.35g.

[0017] By adopting the above technical solution, the present invention has at least the following beneficial effects: The invention provides a hypoeutectoid turnout rail for high-cold areas and a heat treatment production method, which mainly obtains hypoeutectoid structure, adopts 0.50-0.70% C, and takes into account excellent toughness and plasticity while ensuring strength and hardness; adds 0.25≤Cr+V≤0.50, ensures good grain and lamellar spacing refinement effect, improves strength and toughness, and improves the strength and hardness and wear resistance of the turnout rail; at the same time, using the rolling waste heat, based on the temperature change of the turnout rail during the cooling process, adopts a high cooling rate before the phase change, a slow cooling rate during the phase change, and a fast cooling rate after the phase change. It not only improves the phase change supercooling, but also ensures that the structure is pearlite + a small amount of ferrite structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 A schematic diagram of multi-stage heat treatment and step-by-step cooling of a heat treatment production method for hypoeutectoid turnout rails in high-cold regions disclosed in some embodiments of the present invention; Figure 2 A schematic diagram of the sampling position of the tensile specimen and the inspection position of the metallographic specimen in a heat treatment production method for hypoeutectoid turnout rails in high-cold regions disclosed in some embodiments of the present invention; Figure 3 Metallographic photographs of a heat treatment production method for hypoeutectoid turnout rails in high-cold regions disclosed in some embodiments of the present invention. DETAILED DESCRIPTION

[0020] The following is a further detailed description of the embodiments of the present disclosure in conjunction with the accompanying drawings and examples. The detailed description of the following embodiments and the accompanying drawings are used to exemplarily illustrate the principles of the present disclosure, but cannot be used to limit the scope of the present disclosure. The present disclosure can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

[0021] The present disclosure provides these embodiments to make the present disclosure thorough and complete, and to fully express the scope of the present disclosure to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the parts and steps, the composition of the materials, the numerical expressions and the numerical values ​​set forth in these embodiments should be interpreted as being merely exemplary, and not as limiting.

[0022] It should be noted that, in the description of the present disclosure, unless otherwise specified, the meaning of "multiple" is greater than or equal to two; the terms "upper", "lower", "left", "right", "inner", "outer", etc., indicating the orientation or positional relationship, are only for the convenience of describing the present disclosure and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present disclosure. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.

[0023] In addition, the words "first", "second" and similar words used in the present disclosure do not indicate any order, quantity or importance, but are only used to distinguish different parts. "Vertical" does not mean vertical in the strict sense, but is within the tolerance range. "Parallel" does not mean parallel in the strict sense, but is within the tolerance range. "Include" or "comprising" and similar words mean that the elements before the word include the elements listed after the word, and do not exclude the possibility of including other elements.

[0024] It should also be noted that in the description of the present disclosure, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present disclosure can be understood according to the specific circumstances. When a specific device is described as being located between a first device and a second device, there may or may not be an intermediate device between the specific device and the first device or the second device.

[0025] All terms used in the present disclosure have the same meanings as those understood by those of ordinary skill in the art to which the present disclosure belongs, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries, for example, should be interpreted as having meanings consistent with their meanings in the context of the relevant technology, and should not be interpreted in an idealized or extremely formal sense, unless explicitly defined as such herein.

[0026] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered part of the specification.

[0027] The purpose of the present invention is to ensure that the strength and toughness of the hypoeutectoid turnout rails in high-cold areas are improved while greatly improving the corrosion resistance, improving the safety of turnout line operation, and meeting the requirements of turnout rails for railways in high-cold areas. Specifically, it relates to a heat treatment production method for hypoeutectoid turnout rails in high-cold areas, which is designed with a carbon content of 0.50%-0.70%, 0.25%≤Cr+V≤0.50%, 2.5%≤Cu / Ni≤3.5%, and 1.20%≤Si+Mn+P+S≤1.35%. After smelting and casting, the steel billet is heated and rolled into a turnout rail, and the final rolling temperature is 850℃0-950℃; using the residual heat of rolling, an online heat treatment device is used to start cooling at a temperature of 740-850℃, such as Figure 1 As shown, the steel is cooled in 13 stages of heat treatment, with stages 1-3 cooled at 3.0℃ / s -3.5℃ / s, stages 4-6 cooled at 2.5-3.0℃ / s, stages 7-9 cooled at 2.0℃ / s -2.5℃ / s, and stages 10-13 cooled at 1.5℃ / s -2.0℃ / s. The final cooling temperature is 450℃-550℃, and then cooled to room temperature at 2.5℃ / min -3.5℃ / min. Finally, after straightening and processing, the hypoeutectoid turnout rail product for high-cold areas is formed. The smelting process adopts 0.002%-0.010% low sulfur control. The hypoeutectoid turnout rails in high-cold areas produced by this method have a S content of ≤0.008%, a tensile strength of ≥1100MPa, an elongation of ≥12%, a surface hardness of 320-360HB, and a residual stress of ≤250MPa at the bottom of the turnout rails. Compared with the existing U71Mn hot-rolled rails, the relative corrosion resistance is improved by more than 30%, and the wear resistance is improved by more than 35%. It is particularly suitable for turnout rails in high-cold areas.

[0028] The above-mentioned embodiment of the present invention adopts 0.50-0.70%C to obtain a hypoeutectoid structure as the main part, while ensuring the strength and hardness, taking into account the excellent toughness and plasticity. In order to maximize the strength and hardness and wear resistance of the turnout rail, the present invention also adds 0.25≤Cr+V≤0.50, which ensures a good grain and lamellar spacing refinement effect and improves the strength and toughness. Utilizing the residual heat of rolling, based on the temperature change of the turnout rail during the cooling process, a large cooling rate is adopted before the phase change, a slow cooling rate is adopted during the phase change, and a fast cooling rate is adopted after the phase change. It not only improves the supercooling degree of the phase change, but also ensures that the structure is pearlite + a small amount of ferrite structure. The heat treatment start cooling temperature is limited to 740-850℃, the main purpose of which is to limit the large-scale precipitation of proeutectoid ferrite and reduce the comprehensive performance of the turnout rail. The final cooling temperature after heat treatment is limited to 450-550℃, taking into account the phase change characteristics and organizational changes of the entire section. Too low final cooling temperature will lead to the transformation of supercooled austenite into martensite. After heat treatment, the cooling rate is limited mainly because the turnout rail is an asymmetric section. If the cooling rate is too high, the residual stress of the entire section will be too large, which will have an adverse effect on the service of the line. In addition, the present invention limits the control change of the S content in the whole process, mainly considering that sulfur exists in the form of sulfide inclusions in steel, which has an adverse effect on the plasticity, toughness, welding performance, thickness direction performance, fatigue performance and corrosion resistance of steel.

[0029] The present invention is further described below in conjunction with specific embodiments and comparative examples. The heat treatment production method of the hypoeutectoid turnout rail in the high-cold region described in the following embodiments 1-5 is based on the component system of high-speed railway rails. It is designed through Cr / V / Ni components, smelted with low sulfur components, cast and cooled to room temperature, and then heated in a walking-beam heating furnace to an austenite state for a period of time, and then rolled and deformed into the outer dimensions of the turnout rail through a 5-7 frame rail universal rolling mill. The rolled turnout rail utilizes the residual heat of rolling, passes through 13 sections of heat treatment units, and is cooled to 450-550°C at 4 different accelerated cooling rates, and then naturally cooled to room temperature. Finally, the turnout rail described in this patent is processed into a finished rail by a straightening machine and a sawing processing line for shipment. The rails of Examples 1-5 and Comparative Examples 1 and 2 are cast through full-process protection, and preferably use 0.002-0.010% low sulfur control. The chemical composition is shown in Table 1. Examples 1-5 and Comparative Examples 1 and 2 used different heat treatment processes, as shown in Table 2.

[0030] Table 1 Chemical composition of rails in examples and comparative examples (%)

[0031] Table 2 Heating, rolling and heat treatment processes of the examples and comparative examples

[0032] The turnout rails of Examples 1-5 and Comparative Examples 1 and 2 use the same natural cooling and straightening process parameters. According to the requirements of TB / T2344.2-2022 "Steel Rails Part 2: Asymmetric Section Rails for Turnouts", according to the attached Figure 2 Tensile specimen sampling position Process the tensile specimen and inspect it. Figure 2 As shown, the metallographic sample inspection position is carried out for metallographic structure inspection, and the metallographic photos are as attached. Figure 3 The tensile and metallographic data statistics are shown in Table 3.

[0033] Table 3 Mechanical properties of rails in the examples and comparative examples

[0034] Examples 1-5, comparative examples 1 and 2, and U71Mn hot-rolled rail test steel were selected and tested by wet-dry cyclic corrosion test (CCT). The sample was processed into a 10mm10mm4mm thin sheet sample, only one side was exposed for periodic dripping of corrosive liquid, and the other sides were all inlaid with epoxy resin.

[0035] Before the CCT test, the exposed surface of the sample is polished to a bright surface, then cleaned with alcohol in an ultrasonic cleaner, dried with a hair dryer, and placed in a drying oven for later use. The specific process of the CCT test is as follows: (1) Record the initial weight of the sample; (2) Add etching solution to the exposed surface of the sample; (3) Record the weight of the sample, using 0.01 mol / L NaHSO 3 The solution is a corrosive solution; (4) The corrosion time is 40 days; (5) Under the same conditions, the corrosion weight gain of U71Mn hot-rolled rail is 25 mg / cm 2 .

[0036] The results are shown in Table 4.

[0037] Table 4 Rail corrosion performance of examples and comparative examples

[0038] The embodiment and comparative example were selected to carry out wear tests on a wear tester. The wear test parameters were 980N loading force, 100,000 cycles, and the wear loss was measured after the test. The wear loss of U71Mn hot-rolled rail was 0.55g. The results are shown in Table 5.

[0039] Table 5 Rail corrosion performance of examples and comparative examples

[0040] In summary, the hypoeutectoid turnout rail and heat treatment production method for high-cold areas disclosed in the embodiments of the present invention, through reasonable component design, ensures strength while taking into account excellent toughness and plasticity, ensures good grain and lamellar spacing refinement effect, improves strength and toughness, and maximizes the hardness and wear resistance of the turnout rail. By controlling various process parameters of the heat treatment, a high cooling rate is used before the phase transformation, a slow cooling rate is used during the phase transformation, and a fast cooling rate is used after the phase transformation. It not only improves the supercooling degree of the phase transformation, but also ensures that the structure is pearlite + a small amount of ferrite structure. Thereby, a hypoeutectoid turnout rail with strong corrosion resistance suitable for use in high-cold areas is obtained.

[0041] So far, various embodiments of the present disclosure have been described in detail. In order to avoid obscuring the concept of the present disclosure, some details known in the art are not described. Based on the above description, those skilled in the art can fully understand how to implement the technical solution disclosed here.

[0042] Although some specific embodiments of the present disclosure have been described in detail by way of examples, it should be understood by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present disclosure. It should be understood by those skilled in the art that the above embodiments may be modified or some technical features may be replaced by equivalents without departing from the scope and spirit of the present disclosure. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there is no structural conflict.

Claims

1. A heat treatment production method for hypoeutectoid turnout rails in high-cold areas, characterized in that: include: The steel billet after smelting and casting is heated and rolled into a turnout rail; Utilizing the residual heat from rolling, an online heat treatment device is used to cool the steel to the final cooling temperature in a multi-stage heat treatment and step-by-step cooling manner; then cooling to room temperature at a first predetermined rate; After straightening and processing, it is made into hypoeutectoid turnout rail for high-altitude and cold regions.

2. The method for heat treatment production of hypoeutectoid turnout rail in high-cold regions according to claim 1, characterized in that: Calculated by weight percentage, the smelting and casting adopts a composition design of 0.50%-0.70% carbon, 0.25%≤Cr+V≤0.50%, 2.5%≤Cu or Ni≤3.5%.

3. The method for heat treatment production of hypoeutectoid turnout rail in high-cold regions according to claim 1, characterized in that: The final rolling temperature of the steel billet during hot rolling is 850°C-950°C.

4. The method for heat treatment production of hypoeutectoid turnout rail in high-cold regions according to claim 1, characterized in that: The starting temperature of the step-by-step cooling in the multi-stage heat treatment is 740°C-850°C.

5. The method for heat treatment production of hypoeutectoid turnout rail in high-cold regions according to claim 1, characterized in that: The multi-stage heat treatment and step-by-step cooling comprises: The heat treatment was performed in 13 stages with a step-by-step cooling method. Stages 1-3 were cooled at 3.0°C / s -3.5°C / s, stages 4-6 were cooled at 2.5°C / s -3.0°C / s, stages 7-9 were cooled at 2.0°C / s -2.5°C / s, and stages 10-13 were cooled at 1.5°C / s -2.0°C / s.

6. The method for heat treatment production of hypoeutectoid turnout rail in high-cold regions according to claim 1, characterized in that: The final cooling temperature of the multi-stage heat treatment step by step cooling is 450°C-550°C.

7. The method for heat treatment production of hypoeutectoid turnout rail in high-cold regions according to claim 1, characterized in that: In terms of weight percentage, the alloy composition of smelting and casting also includes: 1.20%≤Si+Mn+P+S≤1.35%; Alternatively, the S content of the finished turnout rail is ≤0.008%, and the smelting process adopts 0.002%-0.010% low sulfur control.

8. A hypoeutectoid turnout rail for high-cold areas, characterized in that: The rail is produced by heat treatment production method for hypoeutectoid turnout rail in high-cold regions as described in any one of claims 1 to 7.

9. The hypoeutectoid turnout rail for high-cold regions according to claim 8, characterized in that: The tensile strength is 1105-1212MPa, the elongation is 12%-18%, the surface hardness is 320-360HB; the residual stress at the rail bottom is ≤250MPa.

10. The hypoeutectoid turnout rail for high-cold regions according to claim 8, characterized in that: Using 0.01mol / L NaHSO3 solution as the corrosion solution, the corrosion time is 40 days, and the corrosion weight gain is 9mg / cm 2 -17mg / cm 2 ; Alternatively, with a loading force of 980N, after 100,000 cycles, the wear amount is 0.26g-0.35g.

Citation Information

Patent Citations

  • On-line heat-treated steel rail for high-speed railway and manufacturing method thereof

    CN110607488A

  • Method for improving hardness uniformity of cross section of heat-treated steel rail head

    CN111961810A

  • Production method for improving wear resistance of heat-treated steel rail

    CN113403467A

  • Wear-resistant and corrosion-resistant hypoeutectoid steel rail and production method thereof

    CN113981332A

  • Production method of wear-resistant and corrosion-resistant steel rail for railway in low-temperature region

    CN115466904A

Cited By

  • Turnout steel rail with low rail bottom center residual stress and production method thereof

    CN122012899A

  • Turnout steel rail with uniformly distributed hardness of central section of rail web and production method of turnout steel rail

    CN122012900A

  • Turnout steel rail with uniformly distributed hardness of sections on two sides of railhead and production method thereof

    CN122081628A