Application of modified molecular sieve adsorbent in separation of SF6 / N2 mixture
By modifying the FAU molecular sieve metal cation, the separation performance of the SF6/N2 mixture is improved, and the problems of poor separation selectivity and low adsorption capacity in the prior art are solved, thereby achieving efficient SF6 gas capture and sustainable utilization of resources .
Patent Information
- Application Number
- CN202411167207.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The existing SF6/N2 mixture separation technology has problems such as poor separation selectivity and low adsorption capacity, which leads to waste of resources and environmental pollution of SF6 gas, and the commonly used low-temperature liquefaction or distillation methods have high energy consumption.
By introducing Group IA and Group IIA metal cations to modify the FAU molecular sieve, increase the metal oxide content and improve the separation performance of SF6/N2 mixture, a modified molecular sieve adsorbent was designed for efficient separation of SF6/N2.
The high static adsorption amount and selectivity of SF6 are achieved, the process flow is simplified, and the energy consumption is reduced. The modified molecular sieve material is easy to regenerate under normal temperature and pressure conditions, and has industrial application potential.
Smart Images

Figure CN118904010A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical separation and relates to application of a modified molecular sieve adsorbent in separation of SF6 / N2 mixture. Background Art
[0002] In recent years, with the rapid development of the semiconductor industry, sulfur hexafluoride (SF6), as an excellent etching gas, plays an important role in reactive ion etching and inductively coupled plasma etching technologies of semiconductors such as silicon and carbon silicon with its high selectivity, high etching rate and easy controllability. However, the utilization efficiency of SF6 in the etching process is often less than 60%, and a large amount of unused SF6 gas is discharged into the atmosphere with the purge gas nitrogen (N2). As one of the greenhouse gases banned from emission in the Kyoto Protocol, the global warming potential (GWP) of SF6 is 23,900 times that of CO2, and its life in the atmosphere is as long as 3,200 years. This not only brings environmental problems, but also causes serious waste of resources. Therefore, there is an urgent need for separation technology that can capture and recycle low-concentration SF6 (≤10%) in industrial waste gas, so as to promote its sustainable utilization throughout its life cycle and generate economic benefits while reducing the impact on the environment.
[0003] At present, the most common means of separating SF6 in industry is cryogenic liquefaction or distillation, but these methods often require large energy consumption due to the gas-liquid phase change process involved. In contrast, the adsorption separation method based on porous solid adsorbents has the advantages of high separation efficiency, energy saving, and simple process, and is a very promising SF6 capture method. Among them, high-performance adsorbents are the core of the adsorption separation method, and their design, preparation and optimization are directly related to the efficiency and cost of the method. In recent years, porous adsorbents used for SF6 adsorption separation mainly include metal organic frameworks (MOFs), porous carbon and zeolite molecular sieves. MOFs exhibit high adsorption separation performance due to their high surface area and flexible structural adjustability. However, the high cost and poor structural stability of MOFs limit their large-scale production and further application; porous carbon pores are relatively inert and have fewer polar sites, so their SF6 adsorption capacity and SF6 / N2 selectivity need to be improved; molecular sieve materials have the characteristics of relatively abundant polar sites and good thermodynamic stability, and are a good choice for SF6 separation and recovery. However, existing studies have shown that molecular sieve adsorbents also have the disadvantages of poor separation selectivity and low adsorption capacity for the SF6 / N2 system. Summary of the invention
[0004] In order to solve the above technical problems, considering the significant difference in polarizability between SF6 and N2, the present invention proposes to modify the existing zeolite molecular sieve adsorbent based on thermodynamic effect, and to change the material's ability to interact with SF6 by introducing different metal cations, thereby improving the material's separation performance for SF6 / N2 mixture. While retaining the advantages of simple and low-cost traditional molecular sieve synthesis methods, the adsorbent has extremely high SF6 static adsorption capacity and SF6 / N2 separation selectivity, and can more effectively separate SF6 / N2 mixtures under dynamic conditions, and has the potential for industrial application.
[0005] In order to achieve the above-mentioned purpose of the invention, the present invention provides the following technical scheme: an application of a modified molecular sieve adsorbent in the separation of SF6 / N2 mixture, wherein the adsorbent is a FAU molecular sieve modified with group IA and / or group ⅡA metal cations, and the metal oxide content in the adsorbent is 0.01-30wt%; the modified FAU molecular sieve is applied to the field of SF6 / N2 separation, and the adsorption amount and selectivity of SF6 are greatly improved.
[0006] Group IA metal cations include Li + 、Na + , K + and Cs + One or more of; Group IIA metal cations include Mg 2 + , Ca 2+ and Ba 2+ One or more of the .
[0007] The adsorbent is a FAU molecular sieve modified with group IA and group ⅡA metal cations.
[0008] The FAU molecular sieve is one or more of X molecular sieve, Y molecular sieve and USY molecular sieve.
[0009] The adsorption pressure is 1-10 bar and the adsorption temperature is 0-50°C.
[0010] The volume ratio of SF6 to N2 is 10:90-1:99, and the flow rate of the SF6 / N2 mixture is 2-6 ml / min.
[0011] The regeneration method of the adsorbent comprises the following steps: after the adsorption is completed, regeneration is performed using Ar purge at 25-50°C and normal pressure (1 bar) for 0.5-5 hours or regeneration is performed at 0-500°C and vacuum with an absolute pressure of ≤0.05 bar for 0.5-8 hours. Furthermore, regeneration is performed using Ar purge at normal temperature and pressure (1 bar) for 1-2 hours or regeneration is performed at a vacuum of 0.05 bar for 5-8 hours.
[0012] The preparation method of the adsorbent comprises the following steps:
[0013] S1. Performing ion exchange on FAU molecular sieve with a Group IA metal salt solution and / or a Group IIA metal salt solution;
[0014] The FAU molecular sieve after S2 ion exchange is subjected to solid-liquid separation, washing, drying, calcination and activation to obtain an adsorbent.
[0015] The ion exchange temperature in S1 is 30-90° C., the ion exchange time is 1-5 h, and the ion exchange times are 1-3 times.
[0016] The Group IA metal salt or Group IIA metal salt is one or more of chloride, sulfuric acid and oxalate.
[0017] The concentration of the Group IA metal salt solution or the Group IIA metal salt solution is 0.0025-5 mol / L; the solid-liquid ratio of the FAU molecular sieve to the metal salt solution is 1:5-50 g / mL.
[0018] The calcination temperature is 400-600°C, the calcination time is 3-6h, and the heating rate is 3-5°C / min.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The modified molecular sieve additive prepared by the present invention introduces metal cations to change the cation composition in the pores and the electric field strength inside the molecular sieve, thereby greatly improving the selective adsorption capacity of the pores for SF6 and achieving the adsorption and capture of SF6 at low concentrations.
[0021] 2. The modified molecular sieve additive prepared by the present invention can adsorb SF6 up to 3.56mmol / g, and the IAST selectivity for SF6 / N2 is as high as 600, which has good adsorption selectivity.
[0022] 3. The molecular sieve material of the present invention has a simple preparation process, is green and environmentally friendly, has a high adsorption capacity for sulfur hexafluoride SF6 gas, and has stable chemical properties. The low-concentration SF6 adsorption and capture performance can be fully restored by using Ar purge regeneration for 1-2 hours under normal temperature and pressure (1 bar), further reducing the complexity of the device in actual operation.
[0023] 4. The present invention synthesizes and modifies zeolite molecular sieves and applies them to the field of SF6 selective adsorption and separation for the first time. The obtained modified zeolite sieve exhibits excellent SF6 / N2 gas adsorption and separation performance. Its easy regeneration, excellent structural stability and non-corrosive characteristics have better application prospects in the field of SF6 adsorption and separation than other adsorbents. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1The XRD diffraction patterns of the adsorbent of Example 10 and Comparative Example 1 are shown in FIG.
[0025] Figure 2 Infrared absorption spectra of the adsorbent of Example 10 and Comparative Example 1.
[0026] Figure 3 The adsorbent of Example 10 and Comparative Example 1 were subjected to a total flow rate of 2 mL min at 25 °C, 1 bar, and SF6 / N2 (10:90). -1 Penetration test curve under conditions.
[0027] Figure 4 Example 10: SF6 / N2 (10:90) total flow rate 6 mL min at 25 °C and 1 bar -1 Adsorbent regeneration cycle breakthrough test under conditions.
[0028] Figure 5 This is the SF6 / N2 adsorption isotherm of the adsorbent in Example 10 at 25°C and 1 bar. Specific embodiments
[0029] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0030] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0031] The principles of the molecular sieve adsorbent preparation method provided by the present invention are: the raw materials are efficient and widely available, and the preparation method should be as simple and easy as possible to facilitate industrial production.
[0032] Comparative Example 1
[0033] The synthesis of FAU molecular sieve is referred to (Angew. Chem. Int. Ed., 2022, 61, e202207066). The synthesis method of FAU molecular sieve used in this comparative example is as follows:
[0034] 1. Preparation of zeolite molecular sieve
[0035] Tetraethyl silicate, aluminum isopropoxide, sodium hydroxide and tetraethylammonium hydroxide were mixed in a molar ratio of (1:0.2:0.02:1.2), stirred at room temperature for 2 hours, and then the mixture was placed at 50° C. for 24 hours to obtain a structure directing agent.
[0036] The obtained structure directing agent is mixed with silica sol, sodium aluminate, sodium hydroxide, tetrabutylammonium hydroxide and deionized water in a molar ratio of (3:1:0.033:0.2:0.2:20) to form an initial gel, and the initial gel is stirred at room temperature for 2 hours to form a final gel; the final gel is transferred to an autoclave and crystallized at 120°C for 96 hours to obtain a precipitate containing a molecular sieve.
[0037] After the crystallization is completed, the obtained system is subjected to solid-liquid separation (suction filtration or centrifugal separation), and the obtained solid material is dried at 90°C for 12 hours, placed in a muffle furnace and heated to 600°C at a rate of 2°C / min, and maintained at this temperature for 6 hours to obtain a FAU type molecular sieve.
[0038] Comparative Example 2
[0039] The FAU molecular sieve obtained in Comparative Example 1 was subjected to ion exchange in a 1 mol / L copper nitrate solution; the exchange time was 3 h, the ion exchange temperature was 90° C., the solid-liquid ratio was 1:20 g / ml, the number of ion exchanges was 3 times, and after the ion exchange, centrifugation was performed before the next ion exchange.
[0040] The obtained solid material was dried at 90°C for 12 hours, and then the sample was placed in a muffle furnace and heated to 500°C at a rate of 2°C / min, and this temperature was maintained for 4 hours to obtain the Cu-exchanged FAU molecular sieve.
[0041] Comparative Example 3
[0042] A metal salt solution with a concentration of 1 mol / L was prepared, and the commercial ZSM-5 molecular sieve was placed in the salt solution for ion exchange; the ion exchange time was 3 h, the ion exchange temperature was 90° C., and the solid-liquid ratio was 1:20 g / ml.
[0043] The number of ion exchanges is 3 times, and the metal salt solutions are respectively lithium chloride aqueous solution, lithium chloride aqueous solution and calcium chloride aqueous solution; after the ion exchange, centrifugal separation is performed before the next ion exchange.
[0044] Example 1
[0045] The FAU molecular sieve (obtained in Comparative Example 1) was subjected to ion exchange with an aqueous solution of a Group IA metal salt or an aqueous solution of a Group IIA metal salt, with a solid-liquid ratio of 1:20 g / ml, and the number of ion exchanges was 3. After the ion exchange, centrifugation was performed before the next ion exchange.
[0046] The solid material obtained after the exchange was dried at 90°C for 12 hours, and then the sample was placed in a muffle furnace and heated to 500°C at a heating rate of 2°C / min, and this temperature was maintained for 4 hours to obtain FAU type molecular sieves exchanged with different metals.
[0047] The experimental conditions in each embodiment are specifically shown in Table 1.
[0048] Embodiment 15
[0049] Same as Example 10, but using commercial 13X molecular sieve.
[0050] Example 16
[0051] Same as Example 10, but using commercial NaY type molecular sieve.
[0052] Application Example 1: Evaluating adsorbent performance using fixed bed breakthrough experiments
[0053] 0.5 g of the example adsorbent, comparative example adsorbent, commercial ZSM-5 molecular sieve and commercial SSZ-13 molecular sieve were activated for 6 hours at 300°C and vacuum conditions with an absolute pressure lower than 0.05 bar, and then loaded into adsorption columns. At 298K and 1 bar, a mixed gas of SF6 / N2 (10:90) with a total flow rate of 2 ml / min was passed into the adsorption column. A gas mass spectrometer was connected to the tail end of the adsorption column to detect the gas composition passing through the adsorption column. The adsorption amount and separation time of the gas were finally calculated. When the concentration of N2 and SF6 reached 0.5% of the saturation concentration, it was considered to be penetrated. The results are shown in Table 2. After the adsorbent adsorbed low-concentration SF6, it was regenerated for 40 minutes at 25°C and atmospheric pressure (1 bar) using Ar at a flow rate of 20 ml / min to desorb all SF6 and restore the adsorption performance ( Figure 4 ).
[0054] Figure 3 2 and 3 are the fixed bed breakthrough curves of the samples in Example 10 and Comparative Example 1. The separation effect of the modified Example 10 is significantly better than that before exchange.
[0055] Application Example 2: Adsorbent Static Isotherm Test
[0056] 50±2 mg of the example adsorbent, comparative example adsorbent, commercial ZSM-5 molecular sieve and commercial SSZ-13 molecular sieve were weighed and respectively loaded into the sample tube of the physical adsorption instrument Micromeritics ASAP 2020, and degassed for 6 hours at 300°C and vacuum conditions with an absolute pressure of less than 0.05 bar; the activated sample tube was placed in a constant temperature water bath or an insulation jacket, and high-purity SF6 or N2 gas was filled into the sample tube, and the gas adsorption amount at different equilibrium pressures was measured to obtain the adsorption isotherm. Specific performance is as follows Figure 5 As shown in Table 2.
[0057] in conclusion
[0058] Characterization of the activated adsorbent: Figure 1 It can be seen that the XRD diffraction peak position of the adsorbent in Example 10 is consistent with that of Comparative Example 1, proving that the ion modification does not change the original crystal form of the molecular sieve sample. Figure 2 It can be seen that the infrared absorption peak positions of Example 10 and Comparative Example 1 are consistent, proving that the modified molecular sieve sample still has the same functional groups as the original sample. Figure 3 It can be seen that under the conditions of 298K and 1 bar, in the dynamic penetration test of the raw gas with a total flow rate of SF6 / N2 (10:90) of 2 ml / min, the SF6 penetration time of Example 10 is as high as 168 min, which is twice that of the original molecular sieve sample. Figure 4 It can be seen that the sample of Example 10 can completely restore the low-concentration SF6 adsorption and capture performance by using inert gas (Ar) purge regeneration for 1 hour at room temperature and pressure (1 bar), and the performance is stable after regeneration, and it has the ability to work in a long-term cycle. Static test experiment (Table 2 and Figure 5 ) showed that the adsorption capacity of SF6 by the modified molecular sieve adsorbent at 0.1 bar was 2.84 mmol g -1 The maximum adsorption capacity at 1 bar can reach 3.56 mmol g -1 The IAST selectivity calculated based on the static adsorption capacity at 1 bar is as high as 600, and the selectivity of the SF6 / N2 adsorption ratio is 11.8, which has extremely high SF6 static adsorption capacity and selectivity.
[0059] Table 1 Preparation conditions of the adsorbents in each example
[0060] Adsorbent First exchange Second exchange The third exchange Exchange concentration Exchange temperature Example 1 Lithium chloride Lithium chloride Lithium chloride 1mol / L 90℃ Example 2 Potassium chloride Potassium chloride Potassium chloride 1mol / L 90℃ Example 3 Cesium chloride Cesium chloride Cesium chloride 1mol / L 90℃ Example 4 Calcium chloride Calcium chloride Calcium chloride 1mol / L 90℃ Example 5 Magnesium chloride Magnesium chloride Magnesium chloride 1mol / L 90℃ Example 6 Barium chloride Barium chloride Barium chloride 1mol / L 90℃ Example 7 Lithium chloride Lithium chloride Potassium chloride 1mol / L 90℃ Example 8 Lithium chloride Lithium chloride Calcium chloride 1mol / L 90℃ Example 9 Lithium chloride Lithium chloride Magnesium chloride 1mol / L 90℃ Example 10 Lithium chloride Lithium chloride Barium chloride 1mol / L 90℃ Embodiment 11 Calcium chloride Magnesium chloride Barium chloride 1mol / L 90℃ Example 12 Calcium chloride Calcium chloride Magnesium chloride 1mol / L 90℃ Example 13 Calcium chloride Calcium chloride Barium chloride 1mol / L 90℃ Embodiment 14 Magnesium chloride Magnesium chloride Barium chloride 1mol / L 90℃ Embodiment 15 Lithium chloride Lithium chloride Calcium chloride 1mol / L 90℃ Example 16 Lithium chloride Lithium chloride Calcium chloride 1mol / L 90℃
[0061] Table 2 Adsorption performance of adsorbents in various examples
[0062]
Claims
1. Application of a modified molecular sieve adsorbent in separation of SF6 / N2 mixture, characterized in that: The adsorbent is a FAU molecular sieve modified with group IA and / or group ⅡA metal cations, and the content of metal oxide in the adsorbent is 0.01-30wt%.
2. The use of a modified molecular sieve adsorbent as claimed in claim 1 in the separation of SF6 / N2 mixture, characterized in that: Group IA metal cations include Li + 、Na + , K + and Cs + One or more of the following; Group IIA metal cations include Mg 2+ , Ca 2+ and Ba 2+ One or more of the .
3. The use of a modified molecular sieve adsorbent as claimed in claim 1 in the separation of SF6 / N2 mixture, characterized in that: The FAU molecular sieve is one or more of X molecular sieve, Y molecular sieve and USY molecular sieve.
4. The use of a modified molecular sieve adsorbent as claimed in claim 1 in the separation of SF6 / N2 mixture, characterized in that: The adsorption pressure is 1-10 bar and the adsorption temperature is 0-50°C.
5. The use of a modified molecular sieve adsorbent as claimed in claim 1 in the separation of SF6 / N2 mixture, characterized in that: The volume ratio of SF6 to N2 is 10:90-1:99, and the flow rate of the SF6 / N2 mixture is 2-6 ml / min.
6. The use of a modified molecular sieve adsorbent according to claim 1 in the separation of SF6 / N2 mixture, characterized in that: The regeneration method of the adsorbent comprises the following steps: after the adsorption is completed, regeneration is performed using Ar purge at normal pressure of 25-50° C. for 0.5-5 h or regeneration is performed at vacuum of 0-500° C. and absolute pressure ≤0.05 bar for 0.5-8 h.
7. The use of a modified molecular sieve adsorbent as claimed in claim 1 in the separation of SF6 / N2 mixture, characterized in that: The preparation method of the adsorbent comprises the following steps: S1. Performing ion exchange on FAU molecular sieve with a Group IA metal salt solution and / or a Group IIA metal salt solution; The FAU molecular sieve after S2 ion exchange is subjected to solid-liquid separation, washing, drying, calcination and activation to obtain an adsorbent.
8. The use of a modified molecular sieve adsorbent as claimed in claim 7 in the separation of SF6 / N2 mixture, characterized in that: In the S1, the ion exchange temperature is 30-90° C., the ion exchange time is 1-5 hours, and the number of ion exchanges is 1-3 times.
9. The use of a modified molecular sieve adsorbent as claimed in claim 7 in the separation of SF6 / N2 mixture, characterized in that: The concentration of the IA group metal salt solution or the IIA group metal salt solution is 0.0025-5 mol / L; the solid-liquid ratio of the FAU molecular sieve to the metal salt solution is 1:5-50 g / mL.
10. The use of a modified molecular sieve adsorbent according to claim 7 in separation of SF6 / N2 mixture, characterized in that: The calcination temperature is 400-600° C., and the calcination time is 3-6 hours.
Citation Information
Patent Citations
Method for treating sulphur hexafluoride exhaust gas
CN110124512A
Fluorine-containing greenhouse gas capturing method
CN117160183A
Separation adsorbent for SF6 / N2 mixture and preparation method thereof
CN118287052A
Zeolite adsorbents having a high external surface area and uses thereof
IN201717029306A
Process and zeolitic materials for the separation of gases
US20090288557A1