Fabricated structure joint low-temperature grouting material and quality control method thereof
By using cement-based materials and additives with specific ratios in low-temperature grouting materials, the problems of dry shrinkage, insufficient strength and poor resistance to low-temperature performance of traditional grouting materials under low-temperature conditions are solved, and high strength, crack resistance and adaptation are achieved It is suitable for winter construction and cold areas.
Patent Information
- Application Number
- CN202410982098.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional cement-based grouting materials have large dry shrinkage, insufficient strength, poor low-temperature resistance and small elastic modulus under low temperature conditions, which makes it difficult to effectively follow and absorb the structure during deformation, which may lead to cracks.
The low-temperature grouting formula is adopted including water, gelling materials, sand, gravel, fiber, silicon fume, premature strength agent, expansion agent, anti-cracking agent, antifreeze agent and water reducer, and is controlled by precise proportioning and stirring. Ensure the high strength, crack resistance and adaptability of the grout material, and use additives such as nano-grade silicon fume and wood fibers to improve the performance of the grout material.
It significantly improves the anti-seepage, crack resistance and elastic modulus of grouting materials, can fully fill gaps in negative temperature environments, reduce shrinkage cracks, is suitable for winter construction and cold areas, and reduces construction costs and waiting periods.
Smart Images

Figure BDA0004956376060000041 
Figure BDA0004956376060000051
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building engineering construction, in particular to a low-temperature grouting material for a joint of an assembled structure and a construction method thereof. Background Art
[0002] In order to deal with structural deformation and stress caused by temperature changes, seismic activity or material shrinkage in building or structural design, a spacer is usually preset in the building or structure to withstand a certain degree of movement and deformation, reduce or prevent cracks or damage caused by stress accumulation in the structure, and then grouting is performed in the joints to fill them. Conventional joint grouting materials are usually a mixture of cement-based materials and appropriate admixtures, including cement, sand, water, admixtures and additives. Although this potting material can fill the gaps in concrete structures, there are still the following problems during use: Large drying shrinkage: After pouring, the cement-based material will shrink, which may cause the grouting material to crack or crack after drying. Insufficient strength: If the mixture ratio is not appropriate or the admixture is of poor quality, the strength and durability of the final grouting material may not meet the standards, affecting the stability of the structure. Poor low-temperature resistance: When the temperature is low, the elasticity and ductility of the grouting material deteriorate, making it difficult to effectively follow and absorb the deformation when the structure deforms, thereby increasing the stress inside the structure and possibly causing cracks; Small elastic modulus: Ordinary cement mortar (such as a mixture of ordinary Portland cement and sand) has a small elastic modulus and cannot follow the structural deformation on both sides of the seam, which can easily lead to cracking. Summary of the invention
[0003] The purpose of the present invention is to provide a low-temperature grouting material for joints of assembled structures, so as to solve the technical problems of large drying shrinkage, insufficient strength, poor low-temperature resistance and small elastic modulus of traditional grouting materials under low-temperature conditions.
[0004] To achieve the above purpose, the present invention adopts the following technical solution.
[0005] A low-temperature grouting material for joints of assembled structures comprises water, a cementitious material and sand; it also comprises crushed stone, fiber, silica fume, an early strength agent, an expansion agent, an anti-cracking agent, an antifreeze agent and a water reducing agent; the weight portion of the cementitious material is 40 to 60 parts; the weight portion of the sand is 20 to 40 parts; the weight portion of the crushed stone is 5 to 12 parts; the weight portion of the silica fume is 2 to 6 parts; the weight portion of the fiber is 0.1 to 2 parts; the weight portion of the early strength agent is 0.5 to 3 parts; the weight portion of the expansion agent is 0.1 to 1 part; the weight portion of the anti-cracking agent is 0.1 to 1 part; the weight portion of the antifreeze agent is 0.1 to 1 part; the weight portion of the water reducing agent is 0.1 to 1 part; and the water-to-material ratio is 0.09 to 0.11.
[0006] Preferably, the cementitious material is amorphous calcium aluminate cement, ultra-high strength sulphoaluminate cement or polymer modified cement.
[0007] Preferably, the particle size of the sand is 40-70 mesh, and the particle size of the silica fume is 50nm-700nm.
[0008] Preferably, the crushed stone is made of granite or basalt or a mixture of granite and basalt, and the particle size of the crushed stone is less than or equal to 5 mm.
[0009] Preferably, the early strength agent is sodium chloride or calcium chloride; The water reducer is a wood magnesium water reducer, a melamine water reducer or a polycarboxylic acid water reducer; The antifreeze agent is propylene glycol or chloride salt or nitrate; The anti-cracking agent is polycarboxylate or anti-cracking latex or polypropylene chopped fibers; The water reducer is a wood magnesium water reducer, a melamine water reducer or a polycarboxylic acid water reducer.
[0010] Preferably, the components of the expander include diazonium salts, iminodiacetonitrile, stearic acid esters, lithium bases and alkali metal oxides.
[0011] A quality control method for low-temperature grouting material for joints of assembled structures comprises the following steps.
[0012] Step 1: Raw material selection and quality control; Step 2: Precise control of the proportion: Weigh various raw materials strictly according to the designed proportion to ensure the consistency of each batch of low-temperature grouting materials, and use accurate weighing equipment to avoid human errors. ; Step 3: Control the mixing process: Use mechanical mixing equipment to ensure sufficient mixing time, stirring for 3-5 minutes until there is no dry powder and agglomeration; the mixing order is to add dry materials first, then liquid additives, and finally water to ensure sufficient mixing; Step 4: Quality inspection and control of grouting materials: During the preparation of grouting materials, the appearance quality of the grouting materials is also visually inspected to ensure that there are no cracks or bubbles; samples are taken at different ages for laboratory testing to verify whether the compressive strength, crack resistance, frost resistance index and elastic modulus of the grouting materials meet the design requirements.
[0013] Preferably, the specific method for selecting and controlling the quality of raw materials in step 1 is: Quality control of cementitious materials: testing cementitious materials and ensuring that the quality of cementitious materials meets relevant standards and has good strength and stability; Quality control of fiber quality: select fiber type and length that meet design requirements; Quality control of aggregate quality: the gradation and cleanliness of sand and gravel should meet the standards, without dirt and impurities; Quality control of silica fume: ensure that silica fume is highly active and can improve the density and strength of grouting materials; Quality control of additives: Select high-quality products for early strength agents, expansion agents, anti-cracking agents, antifreeze agents and water reducers to ensure their effectiveness.
[0014] Preferably, when the stirring process is controlled in step three, the temperature of the raw materials is not lower than 5°C, and the temperature of the environment during the stirring process is controlled to be above 5°C.
[0015] Compared with the prior art, the present invention has the following characteristics and beneficial effects.
[0016] 1. In a negative temperature environment, the plastic viscosity of cement-based grouting material increases, and the stirring resistance of the mixer is large, which can easily cause equipment damage, long material mixing time and inability to mix evenly, and at lower temperatures or even negative temperatures, the molecular branches of the water reducer bend and cross-link, resulting in a decrease in the water reduction effect. The present invention appropriately adds silica fume of nanometer size to the grouting material, and its microscopic morphology is a complete sphere. The addition of silica fume accelerates the liquefaction rate of the grouting material and reduces the viscosity of the grouting material, which is very important for ensuring that the grouting material can fully fill and cover the target area during the construction process. At the same time, the addition of silica fume can fill fine cracks and pores, reduce the penetration of water and shrinkage cracks of concrete, and significantly improve the anti-seepage and anti-cracking properties of the grouting material.
[0017] 2. The present invention makes use of the good hydrophilicity of wood fiber to pre-absorb a large amount of water and adhere to the cement slurry. As the water in the cement slurry dissipates, the water in the wood fiber is gradually released, achieving a good water retention effect, and significantly improving the problem of water loss and dry skin on the surface of the grouting material.
[0018] 3. The present invention adds sand and crushed stone aggregates to the grouting material, and replaces sand with crushed stone in a certain ratio. Since crushed stone has lower shrinkage than sand, replacing sand with part of crushed stone can control the shrinkage of concrete, which not only reduces cracks and damage caused by shrinkage, but also improves the compressive strength of the grouting material and reduces costs. In addition, replacing sand with part of crushed stone can also improve the elastic modulus of the grouting material, so that the joint can withstand a certain degree of movement and deformation. At the same time, in order to avoid aggregate extrusion and crushing during mixing, which affects the performance of the grouting material, the present invention controls the particle size of the crushed stone within 5 mm, effectively ensuring the integrity of the crushed stone.
[0019] 4. The present invention adds calcium chloride early strength agent, expansion agent, magnesium chloride antifreeze agent and polycarboxylate water reducer to the grouting material. The use of these additives in the grouting material can not only make the grouting material adapt to the negative temperature environment, but also effectively guarantee the various engineering properties of the grouting material, including strength, durability, crack resistance and construction performance, so that the grouting material is suitable for winter construction or construction in cold areas and long-term stability.
[0020] 5. The negative temperature cement-based grouting material of the present invention can be normally constructed without any additional insulation and maintenance measures. The application of the cold construction scheme can ensure that the grouting material reaches the technical indicators under normal temperature conditions. Under lower temperature conditions, such as around -15°C, it can also meet the technical requirements of prefabricated building connection joints under negative temperature conditions. This plays a key role in shortening the waiting period for winter construction and significantly reducing manpower and equipment costs. DETAILED DESCRIPTION
[0021] This project is a key technology and demonstration for intelligent inspection and supervision of the quality of the main structure of prefabricated concrete buildings. The low-temperature grouting material studied is used to fill the gap between two walls. It is required to have good crack resistance and elastic modulus, be able to withstand a certain degree of movement and deformation, and reduce or prevent cracks or damage caused by stress accumulation in the grouting material. At the same time, since the construction is in winter and located in the colder north, it also has high requirements for its frost resistance. Based on the above design requirements, this application has developed the following low-temperature grouting material.
[0022] Example 1 The low-temperature grouting material for the joints of the assembled structure comprises water, ultra-high-strength sulphoaluminate cement, quartz sand, basalt crushed stone, wood fiber, silica fume, calcium chloride early strength agent, expansion agent, anti-cracking latex, magnesium chloride antifreeze agent and polycarboxylate water reducer; wherein, the weight portion of ultra-high-strength sulphoaluminate cement is 50 parts; the weight portion of quartz sand is 30 parts; the weight portion of basalt crushed stone is 10 parts; the weight portion of silica fume is 4 parts; the weight portion of wood fiber is 1 part, the weight portion of early strength agent is 2 parts; the weight portion of expansion agent is 0.5 parts; the weight portion of anti-cracking latex is 0.5 parts; the weight portion of magnesium chloride antifreeze agent is 0.5 parts; the weight portion of polycarboxylate water reducer is 0.5 parts, and the water-to-material ratio is 0.09.
[0023] In this embodiment, the particle size of the sand is 40-70 mesh, the particle size of the silica fume is 50nm-700nm, and the particle size of the crushed stone is less than or equal to 5mm.
[0024] In this embodiment, the expansion agent is a plastic expansion agent, and the plastic expansion agent SP-B is prepared with diazonium salts and iminodiacetonitrile as the main gas-generating components, stearic acid esters as the stabilizing components, and lithium alkali as the catalyst. A small amount of alkali metal oxide RO is added as an activator and ground together to obtain a plastic expansion agent suitable for low negative temperature conditions.
[0025] Mix cement, fly ash, sand, crushed stone and silica fume evenly; then add early strength agent, expansion agent, anti-cracking agent, antifreeze agent and water reducing agent to the mixed powder in proportion and stir thoroughly; then mix the mixed powder with appropriate amount of water, stir evenly to form grouting material.
[0026] The performance test of the low temperature grouting material prepared in Example 1 is carried out, and the specific test data are shown in Table 1 below: Table 1 Performance index of low temperature grouting materials under negative temperature Example 2 The low-temperature grouting material for the joints of the assembled structure comprises water, ultra-high-strength sulphoaluminate cement, quartz sand, basalt crushed stone, wood fiber, silica fume, calcium chloride early strength agent, expansion agent, anti-cracking latex, magnesium chloride antifreeze agent and polycarboxylate water reducer; wherein, the weight portion of ultra-high-strength sulphoaluminate cement is 40 parts; the weight portion of quartz sand is 35 parts; the weight portion of basalt crushed stone is 12 parts; the weight portion of silica fume is 6 parts; the weight portion of wood fiber is 0.5 parts; the weight portion of calcium chloride early strength agent is 1 part; the weight portion of expansion agent is 1 part; the weight portion of anti-cracking latex is 1 part; the weight portion of magnesium chloride antifreeze agent is 1 part; the weight portion of polycarboxylate water reducer is 1 part, and the water-to-material ratio is 0.10.
[0027] In this embodiment, the expansion agent is a plastic expansion agent, and the plastic expansion agent SP-B is prepared with diazonium salts and iminodiacetonitrile as the main gas-generating components, stearic acid esters as the stabilizing components, and lithium alkali as the catalyst. A small amount of alkali metal oxide RO is added as an activator and ground together to obtain a plastic expansion agent suitable for low negative temperature conditions.
[0028] In this embodiment, the particle size of the sand is 40-70 mesh, the particle size of the silica fume is 50nm-700nm, and the particle size of the crushed stone is less than or equal to 5mm.
[0029] The performance test of the low temperature grouting material prepared in Example 2 is carried out, and the specific test data are shown in Table 2 below: Table 2 Performance index of low temperature grouting material under negative temperature Of course, in other embodiments, the cementitious material may also be amorphous calcium aluminate cement or polymer-modified cement; the crushed stone may also be granite or a mixture of granite and basalt; the early strength agent may also be sodium chloride; the water reducer may also be wood magnesium water reducer or melamine water reducer; the antifreeze agent may also be propylene glycol or nitrate; the anti-cracking agent may also be polycarboxylate or anti-cracking latex or polypropylene chopped fibers; the water reducer may be wood magnesium water reducer or melamine water reducer.
[0030] The quality control method of low-temperature grouting material for joints of assembled structures comprises the following steps.
[0031] Step 1: Raw material selection and quality control.
[0032] Step 2: Precise control of the ratio: Weigh various raw materials strictly according to the designed ratio to ensure the consistency of each batch of low-temperature grouting materials, and use precise weighing equipment to avoid human errors.
[0033] Step three, control the mixing process: use mechanical mixing equipment to ensure sufficient mixing time, stirring for 3-5 minutes, until there is no dry powder and agglomeration; the mixing order is to add dry materials first, then liquid additives, and finally water to ensure sufficient mixing.
[0034] Step 4: Quality inspection and control of grouting materials: During the preparation of grouting materials, the appearance quality of the grouting materials is also visually inspected to ensure that there are no cracks or bubbles; samples are taken at different ages for laboratory testing to verify whether the compressive strength, crack resistance, frost resistance index and elastic modulus of the grouting materials meet the design requirements.
[0035] The specific methods for raw material selection and quality control in step 1 are: Quality control of cementitious materials: testing cementitious materials and ensuring that the quality of cementitious materials meets relevant standards and has good strength and stability; Quality control of fiber quality: select fiber type and length that meet design requirements; Quality control of aggregate quality: the gradation and cleanliness of sand and gravel should meet the standards, without dirt and impurities; Quality control of silica fume: ensure that silica fume is highly active and can improve the density and strength of grouting materials; Quality control of additives: Select high-quality products for early strength agents, expansion agents, anti-cracking agents, antifreeze agents and water reducers to ensure their effectiveness.
[0036] In this embodiment, when the stirring process is controlled in step three, the temperature of the raw materials is not lower than 5° C., and the temperature of the environment during the stirring process is controlled to be above 5° C.
[0037] The above embodiments are not exhaustive of specific implementation methods, and there may be other embodiments. The above embodiments are intended to illustrate the present invention rather than to limit the protection scope of the present invention. All applications derived from simple variations of the present invention fall within the protection scope of the present invention.
Claims
1. A low-temperature grouting material for joints of assembled structures, comprising water, a cementitious material and sand; characterized in that: It also includes crushed stone, fiber, silica fume, early strength agent, expansion agent, anti-cracking agent, antifreeze agent and water reducing agent; the weight portion of the cementitious material is 40 to 60 parts; the weight portion of sand is 20 to 40 parts; the weight portion of crushed stone is 5 to 12 parts; the weight portion of silica fume is 2 to 6 parts; the weight portion of fiber is 0.1 to 2 parts; the weight portion of early strength agent is 0.5 to 3 parts; the weight portion of expansion agent is 0.1 to 1 part; the weight portion of anti-cracking agent is 0.1 to 1 part; the weight portion of antifreeze agent is 0.1 to 1 part; the weight portion of water reducing agent is 0.1 to 1 part; and the water-to-material ratio is 0.09 to 0.
11.
2. The low-temperature grouting material for joints of assembled structures according to claim 1 is characterized in that: The cementitious material is amorphous calcium aluminate cement, ultra-high strength sulphoaluminate cement or polymer modified cement.
3. The low-temperature grouting material for joints of assembled structures according to claim 1 is characterized in that: The particle size of the sand is 40-70 meshes, and the particle size of the silica fume is 50nm-700nm.
4. The low-temperature grouting material for joints of assembled structures according to claim 1, characterized in that: The crushed stone is made of granite or basalt or a mixture of granite and basalt, and the particle size of the crushed stone is less than or equal to 5 mm.
5. The low-temperature grouting material for joints of assembled structures according to claim 1, characterized in that: The early strength agent is sodium chloride or calcium chloride; The water reducer is a wood magnesium water reducer, a melamine water reducer or a polycarboxylic acid water reducer; The antifreeze agent is propylene glycol or chloride salt or nitrate; The anti-cracking agent is polycarboxylate or anti-cracking latex or polypropylene chopped fibers; The water reducer is a wood magnesium water reducer, a melamine water reducer or a polycarboxylic acid water reducer.
6. The low-temperature grouting material for joints of assembled structures according to claim 1, characterized in that: The components of the expander include diazonium salts, iminodiacetonitrile, stearic acid ester, lithium base and alkali metal oxide.
7. A quality control method for low-temperature grouting materials for joints of assembled structures, characterized in that: The steps include: Step 1: Raw material selection and quality control; Step 2: Precise control of the ratio: Weigh various raw materials strictly according to the designed ratio to ensure the consistency of each batch of low-temperature grouting materials, use accurate weighing equipment to avoid human errors; Step 3: Control the mixing process: Use mechanical mixing equipment to ensure sufficient mixing time, stirring for 3-5 minutes until there is no dry powder and agglomeration; the mixing order is to add dry materials first, then liquid additives, and finally water to ensure sufficient mixing; Step 4: Quality inspection and control of grouting materials: During the preparation of grouting materials, the appearance quality of the grouting materials is also visually inspected to ensure that there are no cracks or bubbles; samples are taken at different ages for laboratory testing to verify whether the compressive strength, crack resistance, frost resistance index and elastic modulus of the grouting materials meet the design requirements.
8. The quality control method of low-temperature grouting material for prefabricated structure joints according to claim 7 is characterized in that: The specific methods for raw material selection and quality control in step 1 are: Quality control of cementitious materials: testing cementitious materials and ensuring that the quality of cementitious materials meets relevant standards and has good strength and stability; Quality control of fiber quality: select fiber type and length that meet design requirements; Quality control of aggregate quality: the gradation and cleanliness of sand and gravel should meet the standards, without dirt and impurities; Quality control of silica fume: ensure that silica fume is highly active and can improve the density and strength of grouting materials; Quality control of additives: Select high-quality products for early strength agents, expansion agents, anti-cracking agents, antifreeze agents and water reducers to ensure their effectiveness.
9. The quality control method of low-temperature grouting material for joints of prefabricated structures according to claim 7 is characterized by: When the stirring process is controlled in step three, the temperature of the raw materials is not lower than 5°C, and the temperature of the environment during the stirring process is controlled to be above 5°C.