Method for preparing polyacrylic acid metal salt / AP compound

The composite is formed by reacting sodium polyacrylate water absorption and divalent metals, which solves the problem of nanocatalyst agglomeration, improves the catalytic effect of ammonium perchlorate, and increases the specific surface area by modifying materials, achieving efficient catalysis and simple preparation, solving the problem of solving the problem of The problem of reducing the contact area of ​​the catalyst and complex preparation in the prior art is suitable for industrial applications.

CN118908790APending Publication Date: 2024-11-08SOUTHWEAT UNIV OF SCI & TECH +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410975184.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing nanocatalysts are prone to agglomeration during the catalytic process, resulting in a decrease in the reaction contact area and unable to effectively catalyze the thermal decomposition of ammonium perchlorate. The preparation method of composite materials is complex and expensive, making it difficult to meet industrial production.

Method used

Using the characteristic of extremely strong water absorption of sodium polyacrylate, it instantly absorbs the aqueous ammonium perchlorate solution and reacts with divalent metals to form a composite, and generates metal oxide catalysts in situ to prevent nanocatalyst agglomeration and enhances the contact between the catalyst and ammonium perchlorate. and the polyacrylate metal salt/AP composite is prepared by modifying sodium polyacrylate as a starch-doped fibrous material to further enhance the water absorption and specific surface area.

Benefits of technology

It effectively reduces the high-temperature decomposition peak temperature of ammonium perchlorate, from 451.5℃ to 306.5℃, improves catalytic performance, simplifies the preparation process, reduces costs, and is suitable for industrial promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908790A_ABST
    Figure CN118908790A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a polyacrylic acid metal salt / AP compound, which comprises the following steps: preparing an ammonium perchlorate saturated aqueous solution, adding sodium polyacrylate into the ammonium perchlorate saturated aqueous solution to absorb the ammonium perchlorate saturated aqueous solution, carrying out solid-liquid separation, drying the solid, absorbing the filtrate by using the dried solid, drying, and repeating for multiple times to obtain the polyacrylic acid metal salt / AP compound. Drying the obtained solid until all the ammonium perchlorate saturated aqueous solution is absorbed, so as to obtain a sodium polyacrylate / AP compound; preparing a metal salt solution, adding the sodium polyacrylate / AP compound into the metal salt solution, fully reacting, filtering, washing and drying to obtain the polyacrylic acid metal salt / AP compound. The catalyst and the ammonium perchlorate are prepared into the compound through the sodium polyacrylate, so that agglomeration of the catalyst can be prevented, the contact area of the catalyst and the ammonium perchlorate is increased, and the decomposition peak temperature of the ammonium perchlorate is advanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of energetic material composites, and in particular relates to a method for preparing a polyacrylic acid metal salt / AP composite. Background Art

[0002] Ammonium perchlorate (AP) has good compatibility with solid propellant components and can decompose to produce a large amount of gas when heated. Therefore, it is widely used in solid rocket propellants. It has an excellent oxygen balance value and is an ideal oxidant. The thermal decomposition performance of AP is very sensitive to additives. Transition metals and their oxides are usually used as catalysts to reduce the decomposition temperature of ammonium perchlorate, which can achieve a good catalytic effect. Among them, transition metals include Co, Cu, Ni, etc., and their metal oxides include FeO, NiO, MnO2, MmO4, Co3O4, Cu2O, etc. These nanometals and their oxides can have good catalytic properties for the thermal decomposition of AP, which can reduce the thermal decomposition temperature of AP, increase the heat release, and improve the performance of AP. Researchers reported the catalytic effect of nickel nanocrystals on the thermal decomposition of AP. The results showed that with the addition of NiO nanocrystals, the thermal decomposition temperature of AP decreased (Functional Materials, 2011, 42(03):564-567.); for example, the catalytic activity of different phases of MnO2 nanorods on the thermal decomposition of AP, it was found that the mixed phase MnO2 can significantly reduce the peak thermal decomposition temperature of AP (Rare Metal Materials and Engineering, 2017, 46(03):824-828); through experimental research, green synthesized cobalt oxide nanoparticles (Co3O4 nanoparticles) showed good catalytic activity on the thermal decomposition performance of AP and the combustion performance of propellants (Journal of Catalysis, 2005(12):1073-1077). For example, the study on the batch preparation of nano-CuO and its effect on the thermal decomposition performance of ammonium perchlorate pointed out that 2% nano-CuO has better catalytic performance for AP, which can reduce the high-temperature decomposition temperature of AP with different particle sizes to varying degrees, increase the heat release inappropriately, and increase the reaction rate constant several times (Advancing Technology, 2016, 37(01):188-192).

[0003] However, nanocatalysts also have some shortcomings. For example, they tend to clump together during the catalytic process. When the catalysts clump together, the contact area of ​​the reaction will be reduced. The reactants cannot produce catalytic effects because they cannot contact the catalyst. Therefore, nanocatalysts are generally not used alone for catalysis. Instead, the catalysts are attached to other materials for catalysis. We generally choose two-dimensional or porous materials. The so-called two-dimensional materials refer to a class of materials with a high surface-to-volume ratio, large length and width, and nanometer thickness. They have excellent mass transfer and heat transfer properties and are widely used in many fields. Porous materials are materials with a network-like structure, composed of interconnected or closed pores, such as carbon nanotubes (Acta Physico-Chimica Sinica, 2017, 33(04): 709-728). Studies have shown that the catalytic performance of Cu / CNTs composite particles for AP thermal decomposition is better than that of a simple mixture of Cu, CNTs and AP. This also proves that the catalytic performance of composite materials is better than that of simple composite materials. However, the preparation methods of these materials are generally complicated and expensive, which is difficult to meet the economic requirements and is not conducive to mass production.

[0004] Sodium polyacrylate is a water-soluble polymer compound, non-toxic. It can absorb water several times its own volume. Sodium polyacrylate is divided into low molecular weight, medium molecular weight and high molecular weight, with relative molecular weights ranging from hundreds to tens of millions. The color is generally white or colorless, and the form changes with the change of relative molecular weight, generally powder, liquid or gel. The pH of sodium polyacrylate aqueous solution is generally neutral or weakly alkaline, and its solubility in hydroxide also varies with different metal ions. After sodium polyacrylate encounters calcium hydroxide or magnesium hydroxide, it gradually precipitates as the concentration of metal ions increases, while it is easily soluble in sodium hydroxide. Sodium polyacrylate can form insoluble salts with sufficient divalent or higher metal ions to produce precipitation. However, when there is a small amount of divalent metal ions, it is still a solution and no precipitation will be produced. Summary of the invention

[0005] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.

[0006] In order to achieve these purposes and other advantages according to the present invention, a method for preparing a polyacrylic acid metal salt / AP complex is provided, comprising the following steps:

[0007] Step 1, preparing a saturated aqueous solution of ammonium perchlorate, adding sodium polyacrylate thereto, filtering after the sodium polyacrylate absorbs the saturated aqueous solution of ammonium perchlorate, and drying the solid after solid-liquid separation to obtain a first filtrate and a first composite after drying;

[0008] Step 2, adding the first complex to the first filtrate, filtering after the sodium polyacrylate in the first complex absorbs the first filtrate, drying the solid after solid-liquid separation to obtain a second filtrate and a dried second complex, repeating the above operation multiple times until the sodium polyacrylate completely absorbs all the saturated aqueous solution of ammonium perchlorate, and drying the obtained solid to obtain a sodium polyacrylate / AP complex;

[0009] Step 3: Take a metal salt and add it to a solvent to prepare a metal salt solution, add the sodium polyacrylate / AP complex obtained in step 2 to the metal salt solution, allow it to react fully, filter, wash, and dry to obtain a polyacrylate metal salt / AP complex.

[0010] Preferably, in step 1, the temperature range for preparing the saturated aqueous solution of ammonium perchlorate is 20 to 80°C.

[0011] Preferably, in step 1, the mass ratio of sodium polyacrylate to ammonium perchlorate is 1:10 to 1:100.

[0012] Preferably, in step 1 and step 2, the drying method is one of vacuum drying, freeze drying and supercritical drying.

[0013] Preferably, in the step 1, the time for sodium polyacrylate to absorb the saturated aqueous solution of ammonium perchlorate is 5 to 60 minutes.

[0014] Preferably, in the step 2, the sodium polyacrylate in the first composite absorbs the first filtrate for 5 to 60 minutes.

[0015] Preferably, in step three, the metal salt is a metal salt with a valence of 2 or more, including: copper sulfate, manganese sulfate, ferric sulfate, ferrous sulfate, cobalt sulfate, zinc sulfate, copper acetate, zinc acetate, ferric acetate, cobalt acetate, copper nitrate, nickel nitrate, ferric nitrate, ferrous nitrate, cobalt nitrate hexahydrate, and manganese nitrate.

[0016] Preferably, in step 3, the solvent is one or more of ethanol and ethyl acetate.

[0017] Preferably, in step three, the temperature range for preparing the metal salt solution is 30-50°C.

[0018] Preferably, in step 3, the amount of the metal salt is not less than the amount required for complete reaction between the metal salt and the sodium polyacrylate.

[0019] Preferably, the sodium polyacrylate in step 1 is modified as follows:

[0020] S1, add an auxiliary agent to water, stir evenly, then add sodium polyacrylate, continue stirring evenly to obtain a mixture A;

[0021] S2, dispersing the starch in a buffer solution with a pH of 4.5 to 6.0, heating it in a boiling water bath, and then heating it in an autoclave to obtain a gelatinized starch solution. Then, adding a debranching enzyme thereto, heating it in a warm water bath for enzymolysis, and then heating it in an autoclave to obtain a mixture B;

[0022] S3. Mix mixture A and mixture B evenly and then suck them into a syringe for electrospinning. The upper end of the syringe is facing upward and then dried in a vacuum dryer. Then the spinning needle is connected to the syringe, and electrospinning is performed after setting the electrospinning parameters to finally obtain starch-doped fibrous modified sodium polyacrylate.

[0023] Preferably, in S1, the mass ratio of water, sodium polyacrylate and auxiliary agent is 60-120:1-2:0.5-1, and the auxiliary agent is one or more of methanol, ethanol, n-propanol, 2-propanol, 1,2-propylene glycol, 1,3-propylene glycol and glycerol.

[0024] Preferably, in S2, the buffer solution is an acetic acid-sodium acetate buffer solution, the high pressure sterilization heating temperature is 125-145°C, the heating time is 20-60 min, the debranching enzyme is amylase, the warm water bath heating temperature is 30-60°C, and the enzymatic hydrolysis time is 8-18 h; in S3, the mass ratio of mixture A to mixture B is 6-8:1-2, the vacuum drying temperature is 25-45°C, and the electrospinning parameters are an extrusion speed of the injection pump of 1-3 ml / h, a DC voltage of 5-40 kV, and a spinning time of 1-300 h.

[0025] The invention at least has the following beneficial effects: utilizing the extremely strong water absorption property of sodium polyacrylate, the sodium polyacrylate instantly absorbs an aqueous solution containing energy AP (ammonium perchlorate), and then reacts the aqueous solution with a divalent metal to form a composite, and in situ generates a metal oxide catalyst when heated, which can prevent the agglomeration of the nano catalyst, increase the contact area between the catalyst and ammonium perchlorate, and then efficiently catalyze the ammonium perchlorate. The prepared cobalt polyacrylate / AP composite can advance the high-temperature decomposition peak temperature of AP from the decomposition temperature of 451.5°C to 306.5°C; at the same time, the sodium polyacrylate is modified into a starch-doped fibrous modified sodium polyacrylate, which further increases its water absorption and specific surface area, so that the subsequently prepared polyacrylate metal salt / AP composite has a more excellent catalytic performance for the thermal decomposition of AP; the composite material is simple to prepare, the process is simple, the raw materials are readily available, and it is easy to realize and promote in industry.

[0026] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1The DSC graphs of the raw materials sodium polyacrylate, cobalt polyacrylate and the cobalt polyacrylate / AP complex prepared in Example 1;

[0028] Figure 2 is the XRD pattern of the cobalt polyacrylate / AP composite prepared in Example 1;

[0029] Figure 3 This is the FT-IR graph of the cobalt polyacrylate / AP composite prepared in Example 1. DETAILED DESCRIPTION

[0030] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.

[0031] Example 1

[0032] A method for preparing a polyacrylic acid metal salt / AP complex comprises the following steps:

[0033] Step 1, taking 1.9 g of ammonium perchlorate (AP), stirring at 50° C. to prepare a saturated aqueous solution of ammonium perchlorate, and then adding 0.1 g of sodium polyacrylate thereto, filtering after the sodium polyacrylate absorbs the saturated aqueous solution of ammonium perchlorate for 10 minutes, and vacuum drying the solid after solid-liquid separation to obtain a first filtrate and a first composite after drying;

[0034] Step 2: adding the first complex to the first filtrate, filtering after the sodium polyacrylate in the first complex absorbs the first filtrate for 10 minutes, vacuum drying the solid after solid-liquid separation to obtain a second filtrate and a dried second complex, repeating the above operation multiple times until the sodium polyacrylate completely absorbs all the saturated aqueous solution of ammonium perchlorate, and drying the obtained solid to obtain a sodium polyacrylate / AP complex;

[0035] Step 3: Take 3 g of cobalt nitrate hexahydrate, dissolve it in 100 mL of ethanol at 30° C., stir to prepare a cobalt nitrate solution, then add 1.5 g of the sodium polyacrylate / AP complex prepared in step 2 to it, allow it to react fully, filter, wash and dry to obtain a cobalt polyacrylate / AP complex.

[0036] The thermal decomposition performance of the prepared cobalt polyacrylate / AP composite was tested, and its exothermic peak temperature was 306.5°C.

[0037] Figure 1The DCS diagrams of the raw material AP, the raw material cobalt polyacrylate, and the cobalt polyacrylate / AP complex prepared by this example show that the raw material cobalt polyacrylate has an endothermic peak at 445.2°C, and AP has an endothermic melting peak at 243.1°C. Its low-temperature decomposition peak and high-temperature decomposition peak are 296.7°C and 415.5°C, respectively. The cobalt polyacrylate / AP complex prepared by this example has a reduced endothermic melting peak intensity, only one decomposition peak, and is 109.0°C earlier than the high-temperature decomposition peak. This shows that the catalytic effect of cobalt polyacrylate on AP is obvious. When AP is decomposed at low temperature, cobalt polyacrylate reacts with its low-temperature decomposition product, breaking the low-temperature decomposition reaction equilibrium of AP and allowing the reaction to proceed continuously. Figure 2 This is the XRD diagram of the cobalt polyacrylate / AP composite prepared in this example. It can be seen from the figure that the composite has characteristic diffraction peaks at 19.5°, 22.8°, 24.7°, 27.5°, 30.2°, etc. The position of the characteristic diffraction peak is consistent with the standard card PDF#70-0901 of NH4ClO4, which shows that AP exists in the composite prepared in this example and the crystal form of AP in the composite has not changed. Figure 3 This is the FT-IR image of the cobalt polyacrylate / AP composite prepared in this example. It can be seen from the figure that AP has a wavelength of 1400.3 cm -1 There is an absorption peak at 1083.9cm. It is attributed to the NH bending vibration in the AP molecule. -1 、626.8cm -1 The absorption peak at is ClO4 - Stretching vibration of polyacrylate cobalt at 2920.1cm -1 、2848.7cm -1 、1382.9cm -1 The absorption peaks at 1546.8 cm -1 The peak at is COO - The asymmetric stretching vibration peak of raw material AP and raw material cobalt polyacrylate can be reflected in the cobalt polyacrylate / AP composite, which proves that the composite effect of the two in the composite is good.

[0038] Example 2

[0039] A method for preparing a polyacrylic acid metal salt / AP complex comprises the following steps:

[0040] Step 1, taking 2 g of ammonium perchlorate (AP), stirring at 40° C. to prepare a saturated aqueous solution of ammonium perchlorate, and then adding 0.1 g of sodium polyacrylate thereto, filtering after the sodium polyacrylate absorbs the saturated aqueous solution of ammonium perchlorate for 10 minutes, and vacuum drying the solid after solid-liquid separation to obtain a first filtrate and a first composite after drying;

[0041] Step 2: adding the first complex to the first filtrate, filtering after the sodium polyacrylate in the first complex absorbs the first filtrate for 10 minutes, vacuum drying the solid after solid-liquid separation to obtain a second filtrate and a dried second complex, repeating the above operation multiple times until the sodium polyacrylate completely absorbs all the saturated aqueous solution of ammonium perchlorate, and drying the obtained solid to obtain a sodium polyacrylate / AP complex;

[0042] Step 3: Take 2 g of cobalt nitrate hexahydrate, dissolve it in 100 mL of ethanol at 30° C., stir to prepare a cobalt nitrate solution, then add 1 g of the sodium polyacrylate / AP complex prepared in step 2 to it, allow it to react fully, filter, wash and dry to obtain the corresponding polyacrylate metal salt / AP complex.

[0043] The thermal decomposition performance of the prepared cobalt polyacrylate / AP composite was tested, and its exothermic peak temperature was 308.2°C.

[0044] Example 3

[0045] A method for preparing a polyacrylic acid metal salt / AP complex comprises the following steps:

[0046] Step 1, taking 1.9 g of ammonium perchlorate (AP), stirring at 50° C. to prepare a saturated aqueous solution of ammonium perchlorate, and then adding 0.1 g of sodium polyacrylate thereto, filtering after the sodium polyacrylate absorbs the saturated aqueous solution of ammonium perchlorate for 10 minutes, and vacuum drying the solid after solid-liquid separation to obtain a first filtrate and a first composite after drying;

[0047] Step 2: adding the first complex to the first filtrate, filtering after the sodium polyacrylate in the first complex absorbs the first filtrate for 10 minutes, vacuum drying the solid after solid-liquid separation to obtain a second filtrate and a dried second complex, repeating the above operation multiple times until the sodium polyacrylate completely absorbs all the saturated aqueous solution of ammonium perchlorate, and drying the obtained solid to obtain a sodium polyacrylate / AP complex;

[0048] Step 3: Take 3 g of copper acetate, dissolve it in 100 mL of ethanol at 30° C., stir to prepare a copper acetate solution, add 1.5 g of the sodium polyacrylate / AP complex prepared in step 2, allow it to react fully, filter, wash and dry to obtain a polyacrylate copper / AP complex.

[0049] The thermal decomposition performance of the prepared cobalt polyacrylate / AP composite was tested, and its exothermic peak temperature was 320.4°C.

[0050] Example 4

[0051] The difference between this embodiment and embodiment 3 is that the sodium polyacrylate used in step 1 is modified before being used in step 1, and the modification method is:

[0052] S1. Add 1 g of ethanol to 100 g of water, stir evenly, then add 2 g of sodium polyacrylate, continue stirring evenly to obtain a mixture A;

[0053] S2, dispersing the starch in an acetic acid-sodium acetate buffer solution with a pH of 4.5 to 6.0, heating it in a boiling water bath, and then heating it in an autoclave at 125°C for 30 minutes to obtain a gelatinized starch solution. Then, adding amylase thereto, enzymolyzing it in a 45°C warm water bath for 12 hours, and then heating it in an autoclave at 125°C for 30 minutes to obtain a mixture B;

[0054] S3. Mix 80g of mixture A and 20g of mixture B evenly and then suck them into the syringe for electrospinning. The upper end of the syringe is facing upward, and then it is dried in a vacuum dryer at 30°C. Then, the spinning needle is connected to the syringe. The electrospinning parameters are set as the extrusion speed of the injection pump is 2.5ml / h, the DC voltage is 25kv, and the spinning is 12h, finally obtaining starch-doped fibrous modified sodium polyacrylate.

[0055] The remaining steps are consistent with Example 3. The thermal decomposition performance of the prepared copper polyacrylate / AP composite was tested, and the exothermic peak temperature was 316.5°C.

[0056] Comparative Example 1

[0057] A method for preparing a polyacrylic acid metal salt / AP complex comprises the following steps:

[0058] Step 1, taking 1.9 g of ammonium perchlorate (AP), stirring at 50° C. to prepare a saturated aqueous solution of ammonium perchlorate, and then adding 0.1 g of sodium polyacrylate thereto, filtering after the sodium polyacrylate absorbs the saturated aqueous solution of ammonium perchlorate for 10 minutes, and vacuum drying the solid after solid-liquid separation to obtain a first filtrate and a first composite after drying;

[0059] Step 2: Add the first complex to the first filtrate, wait for the sodium polyacrylate in the first complex to absorb the first filtrate for 10 minutes, then filter, separate the solid and liquid, and vacuum dry the solid to obtain a second filtrate and a dried second complex, repeat the above operation multiple times until the sodium polyacrylate completely absorbs all the saturated aqueous solution of ammonium perchlorate, and dry the obtained solid to obtain a sodium polyacrylate / AP complex.

[0060] The thermal decomposition performance of the prepared sodium polyacrylate / AP composite was tested, and its high-temperature exothermic peak temperature was 410.3°C.

[0061] Comparative Example 2

[0062] A method for preparing a metal salt / AP complex comprises the following steps:

[0063] Step 1: Take 2.0 g of ammonium perchlorate (AP) and stir at 50° C. to prepare a saturated aqueous solution of ammonium perchlorate, then add a saturated aqueous solution containing 0.096 g of copper acetate, and after the copper acetate solution and the saturated aqueous solution of ammonium perchlorate are evenly mixed for 10 minutes, most of the aqueous solution is removed by evaporation and crystallization, and then vacuum drying is performed to obtain a copper acetate / AP complex.

[0064] The thermal decomposition performance of the prepared copper acetate / AP composite was tested, and its high-temperature exothermic peak temperature was 370.0°C.

[0065] Comparative Example 3

[0066] The thermal decomposition performance of the raw material ammonium perchlorate (AP) was tested. The raw material had two thermal decomposition peaks, the high-temperature decomposition peak temperature was 415.5°C, and the low-temperature decomposition peak temperature was 296.7°C.

[0067] From Examples 1 to 3, Comparative Examples 1 to 3 and Figure 1 It can be seen that compared with polyacrylate metal salt / AP complex and sodium polyacrylate, metal salt and raw material AP, sodium polyacrylate has no obvious catalytic effect on AP, the metal salt alone has limited catalytic effect on AP, and polyacrylate metal salt has the most obvious catalytic effect on AP.

[0068] It can be seen from Example 4 that the modified starch-doped fibrous modified sodium polyacrylate can form more polyacrylate metal salt when used to prepare the polyacrylate metal salt / AP composite due to its larger specific surface area and water absorption, thus having a better catalytic effect on AP.

[0069] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.

Claims

1. A method for preparing a polyacrylic acid metal salt / AP complex, characterized in that: The following steps are involved: Step 1, preparing a saturated aqueous solution of ammonium perchlorate, adding sodium polyacrylate thereto, filtering after the sodium polyacrylate absorbs the saturated aqueous solution of ammonium perchlorate, and drying the solid after solid-liquid separation to obtain a first filtrate and a first composite after drying; Step 2, adding the first complex to the first filtrate, filtering after the sodium polyacrylate in the first complex absorbs the first filtrate, drying the solid after solid-liquid separation to obtain a second filtrate and a dried second complex, repeating the above operation multiple times until the sodium polyacrylate completely absorbs all the saturated aqueous solution of ammonium perchlorate, and drying the obtained solid to obtain a sodium polyacrylate / AP complex; Step 3: Take a metal salt and add it to a solvent to prepare a metal salt solution, add the sodium polyacrylate / AP complex obtained in step 2 to the metal salt solution, allow it to react fully, filter, wash, and dry to obtain a polyacrylate metal salt / AP complex.

2. The method for preparing a polyacrylic acid metal salt / AP complex according to claim 1, characterized in that: In the step 1, the temperature range for preparing the saturated aqueous solution of ammonium perchlorate is 20 to 80°C.

3. The method for preparing a polyacrylic acid metal salt / AP complex according to claim 1, characterized in that: In the step 1, the mass ratio of sodium polyacrylate to ammonium perchlorate is 1:10 to 1:

100.

4. The method for preparing a polyacrylic acid metal salt / AP complex according to claim 1, characterized in that: In step 1 and step 2, the drying method is one of vacuum drying, freeze drying and supercritical drying.

5. The method for preparing a polyacrylic acid metal salt / AP complex according to claim 1, characterized in that: In the step 1, the time for sodium polyacrylate to absorb the saturated aqueous solution of ammonium perchlorate is 5 to 60 minutes.

6. The method for preparing a polyacrylic acid metal salt / AP complex according to claim 1, characterized in that: In the step 2, the sodium polyacrylate in the first composite absorbs the first filtrate for 5 to 60 minutes.

7. The method for preparing a polyacrylic acid metal salt / AP complex according to claim 1, characterized in that: In the step 3, the metal salt is a metal salt with a valence of 2 or more, including: copper sulfate, manganese sulfate, ferric sulfate, ferrous sulfate, cobalt sulfate, zinc sulfate, copper acetate, zinc acetate, ferric acetate, cobalt acetate, copper nitrate, nickel nitrate, ferric nitrate, ferrous nitrate, cobalt nitrate hexahydrate, and manganese nitrate.

8. The method for preparing a polyacrylic acid metal salt / AP complex according to claim 1, characterized in that: In the step 3, the solvent is one or more of ethanol and ethyl acetate.

9. The method for preparing a polyacrylic acid metal salt / AP complex according to claim 1, characterized in that: In the step 3, the temperature range for preparing the metal salt solution is 30-50°C.

10. The method for preparing a polyacrylic acid metal salt / AP complex according to claim 1, characterized in that: In the step 3, the amount of the metal salt is not less than the amount required for the complete reaction between the metal salt and the sodium polyacrylate.

Citation Information

Patent Citations

  • Polymeric hydrogel grafted on fibers by calcium ion crosslinking and preparation method thereof

    CN102086592A

  • Micro-nano sodium polyacrylate fiber mat production method

    CN104264235A

  • Method for preparing ammonium perchlorate-metal salt compound based on sodium alginate solidification

    CN107488088A

  • Method for preparing micro-nano fibers through enzymolysis gelatinized starch electrostatic spinning

    CN116949590A

  • Explosive composition

    JP2001181080A