Lithium battery positive electrode dispersing agent, battery positive electrode plate, lithium ion battery and preparation method of lithium ion battery
The lithium battery positive electrode dispersant prepared by polymerization reaction of styrene, maleic anhydride and acrylic monomers was solved, and the preparation process of high solids content and low energy consumption was achieved. , reducing battery manufacturing costs and environmental hazards.
Patent Information
- Application Number
- CN202410984623.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing lithium battery positive electrode materials require a large amount of N-methylpyrrolidone solution during the manufacturing process, resulting in low manufacturing efficiency and increased energy consumption, and it is difficult to achieve high solids content.
The lithium battery positive electrode dispersant prepared by polymerization reaction of styrene, maleic anhydride, acrylic or vinyl acetate monomers is used to form polar solvation chains, improve the dispersion and solid content of the positive electrode material, and reduce the use of NMP solvents. .
The use of NMP solvent is significantly reduced, the solid content of the positive electrode material is increased, the cost of battery manufacturing is saved, and the environmental impact is improved.
Smart Images

Figure CN118909175A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium-ion battery electrode materials, and in particular to a lithium-ion battery positive electrode dispersant, a battery positive electrode sheet, a lithium-ion battery and a preparation method thereof. Background Art
[0002] The development of renewable clean energy such as wind energy, solar energy, and tidal energy has enabled these renewable clean energy sources to be converted into electrical energy for utilization. However, due to the intermittent and unstable electricity generated by the above energy sources, they cannot be directly connected to the power grid for direct utilization. Therefore, storage has become a key to the utilization of renewable clean energy.
[0003] At present, the main electrochemical energy storage solution is the lithium-ion battery solution, but the positive electrode materials of lithium batteries (such as lithium iron phosphate, lithium iron manganese phosphate, etc.) contain nano primary particles and micron secondary particles. When the particle materials are made into electrodes during the battery manufacturing process, a large amount of N-methylpyrrolidone solution is required in the slurry process. NMP is used as a solvent and used together with binders such as polyvinylidene fluoride (PVDF) to form a sol system to ensure the uniformity and consistency of the positive electrode materials. However, this will reduce manufacturing efficiency and increase a lot of energy consumption. Therefore, a dispersant is urgently needed to reduce the amount of N-methylpyrrolidone used in the preparation of lithium battery positive electrodes and achieve a higher solid content slurry. Summary of the invention
[0004] The present application provides a lithium battery positive electrode dispersant, a battery positive electrode sheet, a lithium ion battery and a preparation method thereof to solve the problems existing in the related technologies. The technical solutions are as follows:
[0005] In a first aspect, an embodiment of the present application provides a lithium battery positive electrode dispersant, which is prepared by polymerization reaction of the following monomers;
[0006] The monomer is a composition of styrene, maleic anhydride and a third monomer;
[0007] The third monomer is one or a combination of two or more of acrylic acid monomers, (meth) acrylic acid ester monomers or vinyl acetate.
[0008] In one embodiment, the acrylic monomer is one or a combination of two or more of acrylic acid, methacrylic acid or ethacrylic acid.
[0009] In one embodiment, the (meth)acrylate monomer is any one of ethyl methacrylate, methyl methacrylate, ethyl acrylate, and methyl acrylate, or a combination of two or more thereof.
[0010] In one embodiment, the mass ratio of styrene, maleic anhydride and the third monomer is (4-6): (0.5-2): (2-4).
[0011] In one embodiment, the polymerization reaction is initiated in a solvent by an initiator;
[0012] The solvent is one or a combination of two or more of water, ethanol or N-methylformamide.
[0013] In one embodiment, the initiator is one or a combination of two or more of cumene hydroperoxide, tert-butyl hydroperoxide, benzoyl peroxide, dilauroyl peroxide, tert-butyl perbenzoate or tert-butyl pervalerate.
[0014] In one embodiment, the mass ratio of the total mass of monomers to the added solvent is (1-7):10.
[0015] In one embodiment, the amount of the initiator added is 0.5% to 5% of the total weight of the monomers.
[0016] In one embodiment, the polymerization reaction conditions are: 40-90° C., and the reaction time is 2-20 hours.
[0017] In one embodiment, a dispersant is further added during the polymerization reaction, and the dispersant is one or a combination of two or more of sodium allyl sulfonate, allyloxy nonyl phenoxy propanol polyoxyethylene ether ammonium sulfate or 2-acrylamido-2-methylpropane sulfonic acid.
[0018] In one embodiment, the amount of the dispersant added is 1-10% of the total weight of the monomers.
[0019] In a second aspect, the present invention provides a method for preparing a positive electrode dispersant for a lithium battery, comprising the following steps:
[0020] Add styrene, maleic anhydride and the third monomer into the solvent and mix them evenly;
[0021] In an inert gas atmosphere, the temperature is raised to the reaction temperature, an initiator and a dispersant are added, and an emulsion polymerization reaction is carried out;
[0022] The completely reacted solution is spray-dried to obtain the lithium battery positive electrode dispersant.
[0023] In a third aspect, an embodiment of the present application provides a battery positive electrode sheet, comprising any of the above-mentioned lithium battery positive electrode dispersants.
[0024] In one embodiment, the main material is lithium iron phosphate, and the solid content in the positive electrode sheet is greater than 71.2%.
[0025] In a third aspect, an embodiment of the present application provides a lithium-ion battery, wherein the lithium-ion battery comprises the above-mentioned positive electrode sheet.
[0026] The advantages or beneficial effects of the above technical solution include at least:
[0027] A lithium battery positive electrode dispersant of the present application is obtained by polymerizing monomers including styrene and maleic anhydride and any one of acrylic monomers, (meth) acrylic ester monomers or vinyl acetate; the alternating copolymer of styrene and maleic anhydride is doped with acrylic acid, acrylic ester or vinyl acetate structure to form a polar solvation chain; the polar solvation chain can make fine particles evenly dispersed in the solvent, and increase the solid content of the positive electrode material during slurrying. Among them, styrene and maleic anhydride groups are adsorbed on the surface of the positive electrode material phosphate, and the ring structure brings a steric hindrance effect, increases the distance between fine particles, and improves the dispersibility of the phosphate; the dispersant also changes the charge distribution on the surface of the positive electrode material, so that electrostatic repulsion occurs between particles and reduces agglomeration; the carboxyl group of acrylic acid, the ester group of acrylic ester or vinyl acetate further increases the polarity of the chain and the ability to change the charge distribution; it can reduce the amount of NMP used in the preparation of the positive electrode.
[0028] The above summary is for illustrative purposes only and is not intended to be limiting in any way. In addition to the illustrative aspects, embodiments and features described above, further aspects, embodiments and features of the present application will be readily apparent by reference to the accompanying drawings and the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in the present application and should not be regarded as limiting the scope of the present application.
[0030] Figure 1 This is the electrochemical stability test of the positive electrode slurry of Example 4 and Comparative Example 4. DETAILED DESCRIPTION
[0031] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the present application. Therefore, the drawings and descriptions are considered to be exemplary and non-restrictive in nature.
[0032] With the increasing pressure on environmental protection and cost, the positive electrode slurries on the market are trying to reduce the use of NMP solvent; how to maintain a high solid content while reducing the use of NMP solvent has become one of the problems. In response to the above problems, this application provides a lithium battery positive electrode dispersant, a battery positive electrode sheet, a lithium ion battery and a preparation method thereof.
[0033] The present application embodiment provides a lithium battery positive electrode dispersant, which is prepared by polymerization reaction of the following monomers:
[0034] The monomer is a composition of styrene, maleic anhydride and a third monomer;
[0035] The third monomer is one or a combination of two or more of acrylic acid monomers, (meth) acrylic acid ester monomers or vinyl acetate.
[0036] In the present application, styrene, maleic anhydride and a third monomer of acrylic acid, (meth) acrylic acid ester or vinyl acetate are used as monomers for polymerization reaction to obtain the polymer, wherein styrene and maleic anhydride form alternating polymers, and acrylic acid, acrylic acid ester or vinyl acetate monomers are mixed to form polymer chains.
[0037] The styrene group can better adsorb the polymer on the surface of the positive electrode material; the ring structure of styrene and maleic anhydride increases the distance between the fine particles of the positive electrode material through the steric hindrance effect; and acrylic acid, acrylate or vinyl acetate bring carboxyl and ester groups into the chain, increasing the carbon chain length and chain polarity. The dispersant product has a polar solvation chain that can make the fine particles of the positive electrode material evenly dispersed in the NMP solution, increasing the solid content of the positive electrode material during slurrying. And the dispersant changes the charge distribution on the surface of the positive electrode material, so that electrostatic repulsion occurs between the particles of the positive electrode material, reducing agglomeration. Therefore, the dispersant of the present application can reduce the amount of NMP used in the preparation of the positive electrode material during the preparation of the positive electrode; and increase the solid content.
[0038] In one embodiment, the acrylic monomer is one or a combination of two or more of acrylic acid, methacrylic acid or ethacrylic acid.
[0039] In one embodiment, the (meth)acrylate monomer is any one of ethyl methacrylate, methyl methacrylate, ethyl acrylate, and methyl acrylate, or a combination of two or more thereof.
[0040] In the present application, the alkyl substituents on the acrylic acid and (meth) acrylic acid ester compounds are not long, will not affect the methyl and ester groups, and are helpful for the dissolution of the positive electrode material in the solvent and increase the solid content.
[0041] In one embodiment, the mass ratio of styrene, maleic anhydride and the third monomer is (4-6): (0.5-2): (2-4). When the mass ratio of maleic anhydride to styrene and the third monomer is within the above range, maleic anhydride and the third monomer are nearly alternately polymerized with the styrene monomer, which changes the stability of the polymers of styrene and the third monomer, and styrene and maleic anhydride alone.
[0042] In one embodiment, the polymerization reaction is initiated in a solvent by an initiator;
[0043] The solvent is one or a combination of two or more of water, ethanol or N-methylformamide.
[0044] In one embodiment, the initiator is one or a combination of two or more of cumene hydroperoxide, tert-butyl hydroperoxide, benzoyl peroxide, dilauroyl peroxide, tert-butyl perbenzoate or tert-butyl pervalerate.
[0045] The polymerization reaction is an emulsion polymerization initiated by an initiator. The reaction process can be controlled by the addition of monomers and reaction conditions, and the obtained polymer has stable properties.
[0046] In one embodiment, the mass ratio of the total mass of monomers to the added solvent is (1-7):10.
[0047] In one embodiment, the amount of the initiator added is 0.5% to 5% of the total weight of the monomers.
[0048] In one embodiment, the polymerization reaction conditions are: 40-90° C., and the reaction time is 2-20 hours.
[0049] Under the above reaction conditions, the monomers can be well polymerized and the obtained polymers have excellent properties.
[0050] In one embodiment, a dispersant is further added during the polymerization reaction, and the dispersant is one or a combination of two or more of sodium allyl sulfonate, allyloxy nonyl phenoxy propanol polyoxyethylene ether ammonium sulfate or 2-acrylamido-2-methylpropane sulfonic acid.
[0051] In one embodiment, the amount of the dispersant added is 1-10% of the total weight of the monomers.
[0052] Dispersants can regulate the occurrence of emulsion polymerization reactions, making the polymer formation stable; on the other hand, dispersants do not participate in the occurrence of polymer reactions, so the dispersants can exist completely in the positive electrode dispersant, and act as a dispersant to aid dispersion during the preparation of the positive electrode slurry.
[0053] The present invention provides a method for preparing a positive electrode dispersant for a lithium battery, comprising the following steps:
[0054] Add styrene, maleic anhydride and the third monomer into the solvent and mix them evenly;
[0055] In an inert gas atmosphere, the temperature is raised to the reaction temperature, an initiator and a dispersant are added, and an emulsion polymerization reaction is carried out;
[0056] The completely reacted solution is spray-dried to obtain the lithium battery positive electrode dispersant.
[0057] The preparation process of the present application is emulsion polymerization, which is a mature polymer preparation method, so the preparation process can be prepared on a large scale. In addition, the positive electrode dispersant is spray-dried to form a solid powder, which is different from the existing dispersion. When the positive electrode dispersant of the present application is used, the additional introduction of the solution can be avoided.
[0058] In one embodiment, the inert gas atmosphere is a nitrogen or argon atmosphere.
[0059] An embodiment of the present application provides a battery positive electrode sheet, comprising any one of the above-mentioned lithium battery positive electrode dispersants.
[0060] In one embodiment, the positive electrode sheet includes lithium iron phosphate, acetylene black, polyvinylidene fluoride and the lithium battery positive electrode dispersant of the present application.
[0061] In one embodiment, the main material is lithium iron phosphate, and the solid content in the positive electrode sheet is greater than 71.2%.
[0062] An embodiment of the present application provides a lithium-ion battery, which includes the above-mentioned positive electrode sheet.
[0063] The following is a further description with reference to specific embodiments.
[0064] Example 1
[0065] This example provides a simple method for preparing a positive electrode dispersant for lithium batteries, as follows:
[0066] S1. The nitrogen device, mechanical stirrer, reflux device and three-necked flask were installed, 200g of ethanol was added to the three-necked flask, 20g of styrene, 10g of acrylic acid and 5g of maleic anhydride were added successively, and the mixture was stirred at 100r / min for 10min at room temperature to mix evenly;
[0067] S2. Nitrogen was introduced into the three-necked flask for 10 min, the air in the flask was discharged, the temperature was raised to 60 ° C, 1 g of cumene hydroperoxide and 2 g of sodium allyl sulfonate were added, the stirring speed was adjusted to 300 r / min, and the polymerization time was 6 h;
[0068] S3. The above reaction product is spray dried to control the particle size D50 to 100 um.
[0069] Example 2
[0070] This example provides a simple method for preparing a positive electrode dispersant for lithium batteries, as follows:
[0071] S1. The nitrogen device, mechanical stirrer, reflux device and three-necked flask were installed, 200gN-methylformamide was added to the three-necked flask, 20g styrene, 15g methyl methacrylate and 5g maleic anhydride were added successively, and the mixture was stirred at 100r / min for 10min at room temperature to mix evenly;
[0072] S2. Nitrogen was introduced into the three-necked flask for 10 min, the air in the flask was discharged, the temperature was raised to 90 ° C, cumene hydroperoxide 2 g, allyloxy nonyl phenoxy propanol polyoxyethylene ether ammonium sulfate 0.4 g, the stirring paddle speed was adjusted to 300 r / min, the polymerization time was 2h;
[0073] S3. The above reaction product is spray dried to control the particle size D50 to 100 um.
[0074] Example 3
[0075] This example provides a simple method for preparing a positive electrode dispersant for lithium batteries, as follows:
[0076] S1. The nitrogen device, mechanical stirrer, reflux device and three-necked flask were installed, 150g N-methylformamide and 150g ethanol were added to the three-necked flask, 30g styrene, 10g acrylic acid, 5g maleic anhydride and 10g vinyl acetate were added successively, and the mixture was stirred at 100r / min for 10min at room temperature to mix well;
[0077] S2. Nitrogen was introduced into the three-necked flask for 10 min, the air in the flask was discharged, the temperature was raised to 40 ° C, 1 g of cumene hydroperoxide and 2 g of 2-acrylamido-2-methylpropanesulfonic acid were added, the stirring speed was adjusted to 300 r / min, and the polymerization time was 20 h;
[0078] S3. The above reaction product is spray dried to control the particle size D50 to 50 um.
[0079] Example 4
[0080] This example provides a simple method for preparing a positive electrode dispersant for lithium batteries, as follows:
[0081] S1. After the nitrogen device, mechanical stirrer, reflux device and three-necked flask were installed, 100g of water and 100g of ethanol were added to the three-necked flask, followed by 30g of styrene, 20g of vinyl acetate and 5g of maleic anhydride, and stirred at 100r / min for 10min at room temperature to mix evenly;
[0082] S2. Nitrogen was introduced into the three-necked flask for 10 min, the air in the flask was discharged, the temperature was raised to 55 ° C, 0.275 g of cumene hydroperoxide and 5.5 g of sodium allyl sulfonate were added, the stirring speed was adjusted to 300 r / min, and the polymerization time was 12 h;
[0083] S3. The above reaction product is spray-dried to control the particle size D50 to 10 um.
[0084] Comparative Example 1
[0085] This example provides a simple method for preparing a positive electrode dispersant for lithium batteries, as follows:
[0086] S1. After the nitrogen device, mechanical stirrer, reflux device and three-necked flask were installed, 200 g of ethanol was added to the three-necked flask, followed by 20 g of styrene and 5 g of maleic anhydride, and stirred at 100 r / min for 10 min at room temperature to mix evenly;
[0087] S2. Nitrogen was introduced into the three-necked flask for 10 min, the air in the flask was discharged, the temperature was raised to 60 ° C, 1 g of cumene hydroperoxide and 2 g of sodium allyl sulfonate were added, the stirring speed was adjusted to 300 r / min, and the polymerization time was 6 h;
[0088] S3. The above reaction product is spray dried to control the particle size D50 to 100 um.
[0089] Comparative Example 2
[0090] This example provides a simple method for preparing a positive electrode dispersant for lithium batteries, as follows:
[0091] S1. After the nitrogen device, mechanical stirrer, reflux device and three-necked flask were installed, 200g of ethanol was added to the three-necked flask, followed by 20g of styrene and 10g of acrylic acid, and the mixture was stirred at 100r / min for 10min at room temperature to mix well;
[0092] S2. Nitrogen was introduced into the three-necked flask for 10 min, the air in the flask was discharged, the temperature was raised to 60 ° C, 1 g of cumene hydroperoxide and 2 g of sodium allyl sulfonate were added, the stirring speed was adjusted to 300 r / min, and the polymerization time was 6 h;
[0093] S3. The above reaction product is spray dried to control the particle size D50 to 100 um.
[0094] Comparative Example 3
[0095] This example provides a simple method for preparing a positive electrode dispersant for lithium batteries, as follows:
[0096] S1. The nitrogen device, mechanical stirrer, reflux device and three-necked flask were installed, 200g of ethanol was added to the three-necked flask, 20g of styrene, 10g of acrylic acid and 5g of maleic anhydride were added successively, and the mixture was stirred at 100r / min for 10min at room temperature to mix evenly;
[0097] S2. Nitrogen was introduced into the three-necked flask for 10 min, the air in the flask was discharged, the temperature was raised to 60°C, 1 g of cumene hydroperoxide was added, the stirring speed was adjusted to 300 r / min, and the polymerization reaction time was 6 h;
[0098] S3. The above reaction product is spray dried to control the particle size D50 to 100 um.
[0099] Example 5
[0100] The product obtained in Example 1 was used as a dispersant of 0.2 parts, commercial positive electrode material A nano lithium iron phosphate of 95.5 parts, acetylene black conductive agent of 2 parts, polyvinylidene fluoride binder of 2.5 parts, solvent of 40.5 parts of NMP, and wet pulping was used to prepare positive electrode slurry.
[0101] Comparative Example 4
[0102] The positive electrode slurry was prepared by wet slurrying using 95.5 parts of commercial positive electrode material nano lithium iron phosphate, 2 parts of acetylene black conductive agent, 2.5 parts of polyvinylidene fluoride binder, and 62.3 parts of NMP as solvent.
[0103] Comparative Example 5
[0104] The product obtained in Comparative Example 1 was used as a dispersant of 0.2 parts, commercial positive electrode material nano lithium iron phosphate of 95.5 parts, acetylene black conductive agent of 2 parts, polyvinylidene fluoride binder of 2.5 parts, solvent of 53.0 parts of NMP, and wet pulping was used to prepare positive electrode slurry.
[0105] Comparative Example 6
[0106] The product obtained in Comparative Example 2 was used as a dispersant of 0.2 parts, commercial positive electrode material nano lithium iron phosphate of 95.5 parts, acetylene black conductive agent of 2 parts, polyvinylidene fluoride binder of 2.5 parts, solvent of 49.3 parts of NMP, and wet pulping was used to prepare positive electrode slurry.
[0107] Comparative Example 7
[0108] The product obtained in Comparative Example 3 was used as a dispersant of 0.2 parts, commercial positive electrode material nano lithium iron phosphate of 95.5 parts, acetylene black conductive agent of 2 parts, polyvinylidene fluoride binder of 2.5 parts, solvent of 54.7 parts of NMP, and wet pulping was used to prepare positive electrode slurry.
[0109] The positive electrode slurries of Example 5 and Comparative Example 4 were used to make electrodes. The CV curves were as follows: Figure 1 shown.
[0110] from Figure 1It can be seen that in Comparative Example 4, PVDF is used as the binder of the positive electrode material, and the voltage window of the battery is generally 2 to 4.5 V. In Example 5 of the present application, a dispersant is added to the positive electrode material, and the voltage stability window is wider than that of PVDF. This indicates that during the battery charging and discharging process, the dispersant in the positive electrode material of Example 5 of the present application, like PVDF, will not participate in the electrochemical reaction.
[0111] The solid content of the positive electrode slurries of Example 5 and Comparative Examples 4-7 was tested, and the results are shown in Table 1:
[0112] Table 1 Viscosity and solid content of positive electrode slurry of Example 5 and Comparative Examples 4-7
[0113] LFP PVDF SP Dispersants Viscosity Solid content Increased solid content Comparative Example 4 95.5 2.50 2.00 0.00 13316 61.5% 0.0% Example 5 95.5 2.50 2.00 0.20 13360 71.2% 9.7% Comparative Example 5 95.5 2.50 2.00 0.20 13340 65.4% 5.8% Comparative Example 6 95.5 2.50 2.00 0.20 13402 67% 4.2% Comparative Example 7 95.5 2.50 2.00 0.20 13376 64.7% 6.5%
[0114] From the data in Table 1, it can be seen that the positive electrode slurries prepared in Comparative Example 4 and Example 5 have similar viscosities. Comparative Example 4 uses 62.3 parts of NMP and has a solid content of 61.5%. When Example 5 uses the dispersant prepared in Example 1 of the present application, a positive electrode slurry with similar viscosity is prepared, using only 40.5 parts of NMP, which is 35% less than that in Comparative Example 4; and the solid content of Example 5 reaches 71.2%, which is 9.7% higher than that in Comparative Example 4. This shows that the dispersant of the present application can significantly reduce the use of NMP and can also increase the solid content of the slurry; it also saves the battery manufacturing cost.
[0115] The dispersants in Comparative Examples 5, 6 and 7 of the present application lack a certain component, and the positive electrode slurry with a viscosity similar to that of Comparative Example 4 is prepared. The amount of NMP used is reduced relative to that of Comparative Example 4, but increased relative to Example 5, indicating that the effect of reducing NMP is reduced due to the lack of dispersant components; the same increase in solid content shows the same trend, and the solid content of Comparative Examples 5-6 is increased below 6.5%, which is difficult to achieve when using the dispersant of the present application. The solid content can reach 9.7%.
[0116] In summary, the present application prepares a positive electrode dispersant by polymerization reaction of styrene, maleic anhydride, and any one of acrylic monomers, (meth)acrylate monomers or vinyl acetate, which is used for the preparation of positive electrode slurry, can significantly reduce the use of solvent NMP, and the slurry has a higher solid content; it reduces environmental damage and battery manufacturing costs.
[0117] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are contradictory.
[0118] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0119] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of various changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A lithium battery positive electrode dispersant, characterized in that: Prepared by polymerization reaction of the following monomers: The monomer is a composition of styrene, maleic anhydride and a third monomer; The third monomer is one or a combination of two or more of acrylic acid monomers, (meth) acrylic acid ester monomers or vinyl acetate.
2. A lithium battery positive electrode dispersant according to claim 1, characterized in that: The acrylic monomer is one or a combination of two or more of acrylic acid, methacrylic acid or ethacrylic acid; The (meth)acrylate monomer is any one of ethyl methacrylate, methyl methacrylate, ethyl acrylate, and methyl acrylate, or a combination of two or more thereof.
3. A lithium battery positive electrode dispersant according to claim 1, characterized in that: The mass ratio of styrene, maleic anhydride and the third monomer is (4-6): (0.5-2): (2-4).
4. A lithium battery positive electrode dispersant according to claim 1, characterized in that: The polymerization reaction is initiated in a solvent by an initiator; The solvent is one or a combination of two or more of water, ethanol or N-methylformamide; The initiator is one of cumene hydroperoxide, tert-butyl hydroperoxide, benzoyl peroxide, dilauroyl peroxide, tert-butyl perbenzoate or tert-butyl pervalerate, or a combination of two or more thereof.
5. A lithium battery positive electrode dispersant according to claim 4, characterized in that: The mass ratio of the total mass of monomers to the mass of the added solvent is (1-7): 10; The amount of initiator added is 0.5% to 5% of the total weight of the monomers; The reaction conditions are: 40-90°C, reaction time 2-20h.
6. A lithium battery positive electrode dispersant according to claim 1, characterized in that: A dispersant is also added during the polymerization reaction, wherein the dispersant is one or a combination of two or more of sodium allyl sulfonate, allyloxy nonyl phenoxy propanol polyoxyethylene ether ammonium sulfate or 2-acrylamido-2-methylpropane sulfonic acid; The added amount of the dispersant is 1-10% of the total weight of the monomers.
7. A method for preparing a lithium battery positive electrode dispersant according to any one of claims 1 to 6, characterized in that: The following steps are involved: Add styrene, maleic anhydride and the third monomer into the solvent and mix them evenly; In an inert gas atmosphere, the temperature is raised to the reaction temperature, an initiator and a dispersant are added, and an emulsion polymerization reaction is carried out; The completely reacted solution is spray-dried to obtain the lithium battery positive electrode dispersant.
8. A positive electrode sheet for a battery, characterized in that: A lithium battery positive electrode dispersant comprising any one of claims 1 to 7.
9. The positive electrode sheet of the battery according to claim 8, characterized in that: The main material is lithium iron phosphate, and the solid content in the positive electrode sheet is more than 71.2%.
10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the positive electrode sheet according to claim 9.
Citation Information
Patent Citations
Efficient calcium slurry dispersant and preparation method thereof
CN103468028A
Preparation method of maleic anhydride-styrene-alpha-methylstyrene-vinyl acetate copolymer
CN113402663A
Dispersing agent for lithium ion battery, preparation method of dispersing agent, positive electrode slurry, positive electrode plate and lithium ion battery
CN114583163A
Amphiphilic polymer with comb-shaped structure as well as preparation method and application of amphiphilic polymer
CN116655859A
Aqueous binder for lithium ion battery negative electrode and preparation method of the same
JP2017174804A
Cited By
Sodium-ion battery positive electrode slurry, positive electrode plate, preparation method of positive electrode plate and sodium-ion battery
CN119560504A
A sodium-ion battery positive electrode slurry, a positive electrode sheet, a preparation method thereof and a sodium-ion battery
CN119560504B