Preparation method of rigid polyurethane foam and isocyanate component used by rigid polyurethane foam

By modifying the specific reaction of isocyanate A and polyol components, the preparation method of polyurethane hard bubbles is optimized, and the problem of high thermal conductivity of polyurethane hard bubbles is solved, and the thermal conductivity and fluidity are reduced are achieved, thus reducing the thermal conductivity and stability. Risk of side reactions improves storage stability.

CN118909226APending Publication Date: 2024-11-08HONGBAOLI GRP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411135485.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The thermal conductivity of existing polyurethane hard foams is relatively high, and it is difficult to further reduce while taking into account both fluidity and stability. The environmental protection requirements of the foaming agents used are increased, and the side reaction risks of traditional foaming agents are relatively high.

Method used

Modified isocyanate A is used as isocyanate component, react with specific polyol components, control the reduction amplitude of NCO mass fraction to ≤73%, and use hydroxyl-containing compounds to modify organic isocyanate, combined with appropriate foaming agents and catalysts to optimize The preparation method of polyurethane hard bubbles is to reduce the thermal conductivity.

Benefits of technology

Effectively reduce the thermal conductivity of polyurethane hard bubbles, less than 19mW/(m·K), taking into account fluidity, dimensional stability and mold release stability, reducing side reaction risks, and improving storage stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004999290140000081
    Figure BDA0004999290140000081
  • Figure BDA0004999290140000091
    Figure BDA0004999290140000091
  • Figure BDA0004999290140000092
    Figure BDA0004999290140000092
Patent Text Reader

Abstract

The invention discloses a preparation method of rigid polyurethane foam and an isocyanate component used by the rigid polyurethane foam. The preparation method comprises the following steps: mixing a polyol component with an isocyanate component, and reacting to obtain the rigid polyurethane foam, the isocyanate component contains modified isocyanate A, the modified isocyanate A is organic isocyanate modified by a hydroxyl-containing compound, the organic isocyanate is at least one of diphenylmethane diisocyanate, toluene diisocynate or polymethylene polyphenyl polyisocyanate, and based on the total mass of the isocyanate component, the modified isocyanate A is at least one of diphenylmethane diisocyanate, toluene diisocynate and polymethylene polyphenyl polyisocyanate. The mass ratio of the modified isocyanate A is greater than or equal to 5%. According to the preparation method disclosed by the invention, fluidity, relatively good dimensional stability, demolding stability and compression strength distribution uniformity can be considered, and the prepared rigid polyurethane foam has excellent comprehensive rigid foam performance. The preparation method provided by the invention can effectively reduce the heat conductivity coefficient of the rigid polyurethane foam of the alkane foaming agent system, and the heat conductivity coefficient is less than 19mW / (m.K).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyurethane materials, and in particular relates to a method for preparing polyurethane rigid foam and an isocyanate component used therein. Background Art

[0002] Organic isocyanate is one of the main raw materials for preparing polyurethane rigid foam. It can react with hydroxyl compounds to generate characteristic carbamate chains. Organic isocyanate can also react with other compounds with "active hydrogen" to generate various corresponding chemical chains, thus giving polyurethane materials special properties. At present, the organic isocyanate used in the field of polyurethane rigid foam is mainly polymethylene polyphenyl polyisocyanate, which usually has a functionality of 2.7 and an NCO mass fraction of 31.5%.

[0003] In order to further improve the performance of polyurethane rigid foam, researchers have optimized the isocyanate component. For example, CN110054752B discloses a low-density rigid polyurethane foam and a preparation method thereof, which uses modified isocyanate to improve compatibility with polyol components and improve the stability of polyurethane reaction. In addition, due to the high viscosity of modified isocyanate, butane is used to reduce viscosity, ultimately taking into account low density and excellent foam performance. Although this solution solves the problem of material fluidity, the demoulding stability and thermal conductivity are poor, especially the thermal conductivity is still >19.0mW / (m·K).

[0004] Thermal conductivity is a key indicator for evaluating the thermal insulation performance of polyurethane rigid foam, and it plays a key role in the energy consumption at the user end. Taking household appliances such as refrigerators and freezers as an example, the lower the thermal conductivity of the polyurethane rigid foam used, the better the thermal insulation performance and the less energy consumption required to operate the refrigerator.

[0005] At present, a commonly used method to reduce thermal conductivity is to optimize the composition of the foaming agent. For example, CN111320737B discloses a polyurethane raw material composition, a method for preparing polyurethane rigid foam and its use. It uses a fluoroolefin foaming agent and cyclopentane to form a multi-component foaming agent system, which can reduce the thermal conductivity of the polyurethane rigid foam to 17.9-18.5 mW / (m·K). However, the double bonds of the fluoroolefin foaming agent are unstable and are prone to side reactions with the catalyst in the raw material.

[0006] With the advancement of international environmental protection policies such as the Montreal Protocol and EU F-GAS regulations, the environmental protection requirements for blowing agents are becoming increasingly stringent. Alkanes are still the ideal blowing agent, and for pure alkane blowing agent systems, their thermal conductivity is usually greater than 19mW / (m·K). Therefore, how to further reduce the thermal conductivity while taking into account fluidity and stability is the key in this field. Summary of the invention

[0007] Purpose of the invention: The purpose of the present invention is to provide a method for preparing polyurethane rigid foam and an isocyanate component used therein in view of the deficiencies of the prior art. The present invention further reduces the thermal conductivity of polyurethane rigid foam while taking into account both fluidity and stability.

[0008] Technical solution: The purpose of the present invention is achieved through the following technical solution:

[0009] The invention provides a method for preparing a polyurethane rigid foam, comprising mixing a polyol component and an isocyanate component, and reacting to obtain the polyurethane rigid foam; the polyol component comprises polyether polyol and / or polyester polyol, a foaming agent, a foam stabilizer and a catalyst; the isocyanate component comprises a modified isocyanate A, wherein the modified isocyanate A is an organic isocyanate modified by a hydroxyl compound, wherein the organic isocyanate is at least one of diphenylmethane diisocyanate, toluene diisocyanate or polymethylene polyphenyl polyisocyanate, and the NC of the organic isocyanate is 1. O% is N1, the NCO% of the modified isocyanate A is N2, (1-N2 / N1)×100%≤73%; based on the total mass of the isocyanate component, the mass proportion of the modified isocyanate A is ≥5%, such as 5-100%; the average hydroxyl value of the polyol component when not containing a foaming agent is 330-480 mgKOH / g, and the average functionality is ≥3.5; the NCO% of the isocyanate component is 17.0-31.3%, preferably 17.0-30.5%; the average functionality is ≥2.2, preferably 2.4-3.0.

[0010] The present invention uses a specific polyol component and a specific isocyanate component to react to obtain a polyurethane rigid foam with excellent properties. The special feature of the raw materials used in the present invention is that a modified isocyanate A with a NCO mass fraction reduction of ≤73% is used as one of the isocyanate components, and the total NCO% of the isocyanate component is limited to 17.0-31.3%, and the average functionality is ≥2.2. The average hydroxyl value of the polyol component matched therewith is 330-480 mgKOH / g when no blowing agent is present, and the average functionality is ≥3.5. Studies have found that the above raw materials work synergistically with each other, which can effectively reduce the thermal conductivity, while taking into account the material fluidity and dimensional stability.

[0011] The modified isocyanate A of the present invention is to react a hydroxyl-containing compound with an organic isocyanate to reduce the NCO mass fraction, thereby obtaining a modified isocyanate A with a changed structure, functionality and NCO%. The NCO% of the modified isocyanate A is ≤28%, such as 13-28%, preferably 18.0-25.0%. The hydroxyl-containing compound used is usually a polyether polyol, polyester polyol, a small molecule alcohol, etc., with an average functionality ≥2, such as any value between 2 and 3, as long as the purpose of the modification of the present invention can be achieved. (1-N2 / N1)×100% represents the reduction in the NCO mass fraction before and after the modification. Controlling the reduction in the NCO mass fraction to ≤73% can not only take into account the fluidity of the material, but also be more conducive to the formation, stability and distribution of bubble nuclei, and optimize the thermal conductivity and dimensional stability. For different types of organic isocyanates, the minimum value of the reduction of the NCO mass fraction is different. For example, for modified toluene diisocyanate, the reduction of the NCO mass fraction is preferably greater than 41%, such as 41.9% to 73.0%, and more preferably 48.5% to 65.0%; for modified diphenylmethane diisocyanate, the reduction of the NCO mass fraction is preferably greater than 16.5%, such as 25.4% to 73%, and more preferably 28% to 60%; for modified polymethylene polyphenyl polyisocyanate, the reduction of the NCO mass fraction is preferably greater than 9%, such as 18% to 73%, and more preferably 20% to 60%. That is, the preferred reduction of the NCO mass fraction of the present invention is 18% to 73%, and more preferably 20% to 65%.

[0012] The isocyanate component used in the present invention has an NCO% of less than 31.5% (NCO% is 17.0-31.3%), which matches the polyol component with an average functionality of ≥3.5, and can better stabilize the foaming process and maintain the balance of various properties of the rigid foam.

[0013] The polyol component of the present invention generally contains polyether polyol and / or polyester polyol, a foaming agent, a foam stabilizer and a catalyst. In addition, in order to increase the functionality of the polyurethane rigid foam, various additives may be added, such as inorganic fillers, flame retardants, colorants, nucleating agents, etc., wherein the specific types and proportions of each raw material are well known in the art, as long as the average hydroxyl value of the polyol component in the absence of a foaming agent is 330 to 480 mgKOH / g, and the average functionality is ≥3.5, it can be used in the present invention. Among them, the foaming agent may be a physical foaming agent and / or a chemical foaming agent, and the chemical foaming agent is generally water, but other new chemical foaming agents that can generate gas by reaction are not excluded. The usage ratio of the polyol component to the isocyanate component is usually determined according to the isocyanate index, which is the ratio of the molar amount of the reactive group (i.e., NCO group) in the isocyanate component to the molar amount of the reactive group (i.e., OH group) in the polyol component. The ratio can be conventional in the art. For example, the applicable ratio range of the present invention can be 1.03 to 1.40. The usage of the blowing agent is determined according to the target core density of the rigid polyurethane foam and the solubility of the blowing agent in the polyol component. The specific type and proportion of the blowing agent can also be conventional in the art.

[0014] In order to take into account both dimensional stability and demoulding stability, the modified isocyanate A is preferably an organic isocyanate modified by a hydroxyl compound containing a ring-containing polyol. The ring-containing polyol is a polyol with an aromatic ring and / or an alicyclic ring in its molecular structure, and can be a ring-containing polyether polyol and / or a ring-containing polyester polyol. The ring-containing polyether polyol can be a Mannich polyether polyol, a polyether polyol with an aromatic amine compound as an initiator (such as o-toluenediamine-based polyether polyol), a polyether polyol with an aminocycloalkanol as an initiator (such as 2-aminocyclohexanol-based polyether polyol), a polyether polyol with an alicyclic diamine (such as cyclohexanediamine) as an initiator, a polyether polyol with an alicyclic diol (such as cyclohexanediol) as an initiator, a polyether polyol with an epoxy cycloalkane (such as epoxy cyclohexane) as a polymerization monomer, etc.; the ring-containing polyester polyol can be an aromatic polyester polyol, such as a benzene ring-containing polyol substance obtained by depolymerization of polyethylene terephthalate, an aromatic polyester polyol obtained by reacting an aromatic dicarboxylic acid (or anhydride) with a polyol, wherein the aromatic dicarboxylic acid (or anhydride) can be selected from phthalic anhydride, terephthalic acid, isophthalic acid or dimethyl terephthalate.

[0015] It is further preferred that the average functionality of the ring-containing polyol is ≥ 2, and it is further preferred that the modified isocyanate A is an organic isocyanate modified by a hydroxyl compound containing an aromatic polyester polyol, such as an organic isocyanate modified by a hydroxyl compound containing a phthalic anhydride polyester polyol. The organic isocyanate modified by the ring-containing polyol can not only improve the compatibility with the polyol component of the present invention, but also give the modified isocyanate A specific properties, so that it maintains the stability of the bubble core and takes into account the strength of the foam. In particular, when the 25°C viscosity of the modified isocyanate A is greater than 1000mPa·s, such as 1200-17000mPa·s, and the average functionality is 2.0-2.6, the comprehensive performance of the obtained polyurethane rigid foam is better. More preferably, when the 25°C viscosity of the modified isocyanate A is ≥2500mPa·s, the improvement effect on the thermal insulation performance is best, especially when the 25°C viscosity is ≥3400mPa·s, the demolding stability can be further taken into account, but the viscosity should not be too high. Preferably, the 25°C viscosity of the modified isocyanate A is 2500-17000mPa·s to take into account the fluidity.

[0016] The isocyanate component of the present invention may contain other isocyanate types in the art in addition to the modified isocyanate A, as long as the NCO% of the isocyanate component is 17.0 to 31.3% and the average functionality is ≥2.2.

[0017] In order to further improve the demoulding stability of the polyurethane rigid foam, the present invention further preferably comprises the isocyanate component consisting of modified isocyanate A and polymethylene polyphenyl polyisocyanate, wherein the average functionality of the polymethylene polyphenyl polyisocyanate is generally 2.6 to 3.0, more preferably 2.7 to 3.0, and even more preferably 2.9 to 3.0. Based on the total mass of the isocyanate component, the mass proportion of polymethylene polyphenyl polyisocyanate is ≥ 75%, that is, the mass proportion of modified isocyanate A is ≤ 25%, and it is further preferred that the mass proportion of modified isocyanate A is 10% to 25%.

[0018] In addition, in order to achieve specific functionality, the isocyanate component of the present invention may also contain modified isocyanate A, polymethylene polyphenyl polyisocyanate and inert auxiliary agents at the same time. The inert auxiliary agents are substances that do not react with organic isocyanates, such as physical foaming agents, fluorine-containing compounds, silicone compounds, etc., and their usage can be based on the conventional amount in the art.

[0019] As another effective method for maintaining the stability of the bubble nucleus, the viscosity of the isocyanate component at 25° C. is greater than 500 mPa·s, such as 500 to 1500 mPa·s, and more preferably 500 to 1200 mPa·s.

[0020] In order to improve the uniformity of cell distribution and obtain a better compression strength distribution, it is further preferred that the viscosity difference between the polyol component and the isocyanate component at 25°C is ≤700mPa·s, and further preferably ≤500mPa·s. The viscosity of the polyol component and the isocyanate component will be affected by composition and environmental changes. At different time points, the viscosity of the two components is usually different. The key to the performance of polyurethane rigid foam lies in the viscosity value of the two components when they are about to be mixed. The viscosity difference of the present invention is the viscosity difference between the polyol component and the isocyanate component at 25°C before they are about to be mixed.

[0021] In order to improve the mixing effect, especially when the viscosity of the polyol component and / or the isocyanate component at 25°C is ≥450 mPa·s, it is further preferred that the mixing pressure is 120-160 bar, and the pressure increase can be achieved by a mixing gun head of a high-pressure foaming machine.

[0022] The foaming agent of the present invention can use a known foaming agent in the art, such as a chemical foaming agent can be selected from water, and a physical foaming agent can be selected from one or more of an alkane foaming agent, a hydrofluorocarbon foaming agent, a fluoroolefin foaming agent, carbon dioxide, and methyl formate.

[0023] The present invention can effectively reduce the thermal conductivity of the alkane foaming system. Therefore, it is preferred that the foaming agent contains a physical foaming agent and the physical foaming agent preferably contains an alkane compound, such as an alkane with a boiling point of -45°C to 100°C, which can be selected from at least one of cyclopentane, isopentane, neopentane, n-pentane, n-butane, isobutane, cyclohexane, propane, n-hexane and its isomers, n-heptane and its isomers, etc.

[0024] In order to better match the isocyanate component of the present invention and exert a better synergistic effect, it is preferred that the average functionality of the polyol component is 3.5 to 5.0.

[0025] More preferably, the average hydroxyl value of the polyol component without a blowing agent is 350 to 460 mgKOH / g.

[0026] The present invention also provides an isocyanate component, which contains modified isocyanate A, wherein the modified isocyanate A is an organic isocyanate modified by a hydroxyl compound, wherein the organic isocyanate is at least one of diphenylmethane diisocyanate, toluene diisocyanate or polymethylene polyphenyl polyisocyanate, the NCO% of the organic isocyanate is N1, the NCO% of the modified isocyanate A is N2, and (1-N2 / N1)×100%≤73%; based on the total mass of the isocyanate component, the mass proportion of the modified isocyanate A is ≥5%, the NCO% of the isocyanate component is 17.0-31.3%, preferably 17.0-30.5%, and the average functionality is ≥2.2, preferably 2.4-3.0.

[0027] In order to achieve both dimensional stability and demolding stability, the modified isocyanate A is preferably an organic isocyanate modified with a hydroxy compound containing a ring-containing polyol.

[0028] It is further preferred that the modified isocyanate A is an organic isocyanate modified by a hydroxyl compound containing an aromatic polyester polyol, that is, as long as a ring-containing polyol, especially an aromatic polyester polyol, is used in the process of modifying the organic isocyanate, a beneficial effect is achieved. Therefore, the present invention does not limit the specific mass proportion of the ring-containing polyol in the hydroxyl compound, which can be >10%, 100%, or any value between 10 and 100%. In particular, when a ring-containing polyol is used and the 25°C viscosity of the obtained modified isocyanate A is >1000mPa·s and the average functionality is 2.0 to 2.6, the comprehensive performance of the obtained polyurethane rigid foam is better.

[0029] In order to further improve the optimization effect on the pore morphology and distribution, the isocyanate component of the present invention preferably consists of modified isocyanate A and polymethylene polyphenyl polyisocyanate, wherein the average functionality of the polymethylene polyphenyl polyisocyanate is preferably 2.6 to 3.0, more preferably 2.7 to 3.0, and further preferably 2.9 to 3.0; based on the total mass of the isocyanate component, the mass proportion of modified isocyanate A is ≤25%.

[0030] Beneficial effects:

[0031] (1) The preparation method of the present invention can take into account fluidity, good dimensional stability, demoulding stability and uniformity of compression strength distribution, and the prepared polyurethane rigid foam has excellent comprehensive rigid foam properties;

[0032] (2) The preparation method of the present invention can effectively reduce the thermal conductivity of polyurethane rigid foam in an alkane foaming agent system, and the thermal conductivity is less than 19mW / (m·K);

[0033] (3) The preparation method of the present invention does not require the addition of additional fluoroolefin substances, and can obtain a lower thermal conductivity, reduce the risk of side reactions, and have better storage stability. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is described in detail below through specific embodiments, but the protection scope of the present invention is not limited to the embodiments.

[0035] Some of the raw materials used in the present invention are as follows:

[0036] (1) The NCO% of polymethylene polyphenyl polyisocyanate is usually 30.0-32.0%, and the functionality is usually 2.6-3.0. The polymethylene polyphenyl polyisocyanate used in the embodiment of the present invention is: M20s, nominal NCO% 31.5%, nominal functionality 2.7, purchased from BASF; 44V20L, nominal NCO% 31.5%, nominal functionality 2.6, purchased from Covestro; 44V40L, nominal NCO% 32.0%, nominal functionality 2.8, purchased from Covestro; PAPI TM 580N, nominal NCO% 30.8%, nominal functionality 3.0, purchased from Dow; 2085, nominal NCO% 30.5%, nominal functionality 2.9, available from Huntsman.

[0037] (2) Modified isocyanate A

[0038] A-1#, homemade, made by modifying 4,4'-MDI (CAS No.: 101-68-8) with glycerol polyether H307, with a NCO mass fraction reduction of 46.3%, NCO% = 18%, an average functionality of 2.35, and a viscosity of 3012 mPa·s at 25°C;

[0039] A-2#, homemade, using aromatic polyester polyols with a mass ratio of 1:9 PS-2602 and diethylene glycol based polyether polyol VORANOL TM 220-110 modified M20s was prepared, with a NCO mass fraction reduction of 20.6%, NCO% = 25%, an average functionality of 2.56, and a viscosity of 1403 mPa·s at 25°C;

[0040] A-3#, homemade, made from cyclohexanediol-based polyether polyol Y-1# modified TDI-80 (Covestro), with a NCO mass fraction reduction of 73.0%, NCO% = 13%, an average functionality of 2.27, and a viscosity of 4604 mPa·s at 25°C;

[0041] A-4#, self-made, made from isophthalic acid-based polyester polyol Y-2# modified TDI-80, with a NCO mass fraction reduction of 64.7%, NCO% = 17%, an average functionality of 2.22, and a viscosity of 4319 mPa·s at 25°C;

[0042] A-6#, homemade, using aromatic polyester polyol PS-2502A modified TDI-80, NCO mass fraction reduced by 41.9%, NCO% = 28%, average functionality of 2.0, 25℃ viscosity of 1200mPa·s;

[0043] A-7#, homemade, made from isophthalic acid-based polyester polyol Y-2# modified TDI-80, NCO mass fraction reduced by 58.5%, NCO% = 20%, average functionality of 2.17, 25℃ viscosity of 3426mPa·s;

[0044] A-8#, homemade, using aromatic polyester polyol PS-2352 modified TDI-80, NCO mass fraction reduced by 62.7%, NCO% = 18%, average functionality of 2.0, 25℃ viscosity of 3628mPa·s;

[0045] A-9#, homemade, modified with aromatic polyester polyol HF-8730 M20s was prepared, with a NCO mass fraction reduction of 27.0%, NCO% = 23%, an average functionality of 2.41, and a viscosity of 11234 mPa·s at 25°C;

[0046] A-10#, homemade, made from aromatic polyester polyol HF-86304 modified TDI-80, NCO mass fraction reduced by 48.5%, NCO% = 24.8%, average functionality of 2.0, 25℃ viscosity of 7629mPa·s;

[0047] A-11#, homemade, modified with aromatic polyester polyol HF-8020 M20s was obtained, with a NCO mass fraction reduction of 23.8%, NCO% = 24.0%, an average functionality of 2.5, and a viscosity of 16983 mPa·s at 25°C;

[0048] A-12#, homemade, made from aromatic polyester polyol PS-2352 modified TDI-80, NCO mass fraction reduced by 52.3%, NCO% = 23.0%, average functionality of 2.0, 25℃ viscosity of 2517mPa·s;

[0049] DA-2#, homemade, using aromatic polyester polyol PS-2502A modified TDI-80, NCO mass fraction reduced by 79.3%, NCO% = 10.0%, average functionality of 2.0, 25℃ viscosity of 4137mPa·s;

[0050] DA-5#, homemade, using aromatic polyester polyol PS-2502A Modification M20s was obtained, with a NCO mass fraction reduction of 8.3%, NCO% = 28.9%, an average functionality of 2.63, and a viscosity of 869 mPa·s at 25°C;

[0051] The preparation method of modified isocyanate A is as follows: vacuum dehydrating a hydroxyl-containing compound, and then reacting it with an organic isocyanate at 40-70° C. to obtain the modified isocyanate A after the reaction is completed.

[0052] (3) Polyol component, including polyether polyol, polyester polyol, catalyst, foam stabilizer, physical foaming agent and water, all purchased from Hongbaoli:

[0053] H9506, average functionality is 5.0, average hydroxyl value is 332mgKOH / g, viscosity at 25℃ is 683mPa·s, water content is 2.2wt%, and the physical foaming agent is cyclopentane, with a content of 13.0wt%;

[0054] H9585.3, average functionality is 4.8, average hydroxyl value is 351mgKOH / g, viscosity at 25℃ is 572mPa·s, water content is 2.3wt%, physical foaming agent is cyclopentane, content is 13.8wt%;

[0055] H9557.1, average functionality is 3.5, average hydroxyl value is 479mgKOH / g, viscosity at 25℃ is 718mPa·s, water content is 2.5wt%, physical foaming agent is cyclopentane, content is 14.5wt%;

[0056] H9683, average functionality is 3.8, average hydroxyl value is 460mgKOH / g, viscosity at 25℃ is 357mPa·s, water content is 2.2wt%, physical foaming agents are cyclopentane and isopentane, the contents are 9.5wt% and 4.3wt%, respectively;

[0057] H9537.1, average functionality is 4.3, average hydroxyl value is 380mgKOH / g, viscosity at 25℃ is 702mPa·s, water content is 2.2wt%, physical foaming agent is cyclopentane, content is 13.0wt%;

[0058] H9584, average functionality is 3.8, average hydroxyl value is 408mgKOH / g, viscosity at 25℃ is 452mPa·s, water content is 2.3wt%, and the physical foaming agent is cyclopentane, with a content of 13.8wt%;

[0059] H9524, average functionality is 3.2, average hydroxyl value is 310 mgKOH / g, viscosity at 25°C is 468 mPa·s, water content is 2.2 wt%, and the physical foaming agent is cyclopentane, with a content of 13.8 wt%.

[0060] (4) Other raw materials

[0061] Phthalic anhydride polyester polyol, PS-2352, PS-2502A, PS-2602, all purchased from Stepan; phthalic anhydride polyester polyols, HF-8730, HF-86304, HF-8020, all purchased from Huafeng Group; cyclohexanediol-based polyether polyol Y-1#, homemade, hydroxyl value of 307 mgKOH / g, average functionality of 2.3; isophthalic acid-based polyester polyol Y-2#, homemade, hydroxyl value of 402 mgKOH / g, average functionality of 2.3; glycerol polyether, H307, purchased from Hongbaoli; diethylene glycol polyether, VORANOL TM 220-110, purchased from Dow; organic silicone oil Niax TM Silicone L6891, purchased from Momentive;

[0062] The method for preparing the aromatic polyester polyol is as follows: subjecting aromatic carboxylic acid and glycerol to a condensation reaction at 140-200° C. with an average functionality of 2.3, and obtaining the aromatic polyester polyol after removing water, small molecular byproducts and excess reaction raw materials.

[0063] The preparation method of cyclohexanediol-based polyether polyol is as follows: cyclohexanediol and glycerol are added into a reaction kettle according to an average functionality of 2.3, the reaction kettle is replaced with an inert gas and vacuumized, and the kettle temperature is maintained at 100-180°C after the vacuumization is stopped, a mixture of propylene oxide and ethylene oxide is added, and a crude polyether product is obtained after the reaction is completed, and the polyether polyol is obtained after refining treatment.

[0064] The specific compositions of the isocyanate components used in Examples 1 to 12 and Comparative Examples 1 to 5 of the present invention are shown in Table 1 and Table 2.

[0065] Table 1 Specific composition of isocyanate components S-1# to S-9#

[0066]

[0067]

[0068] Table 2 Specific composition of S-10#~DS-5# isocyanate components

[0069]

[0070] The method for preparing the rigid polyurethane foam in the embodiments and comparative examples of the present invention is as follows:

[0071] (1) Preparation of isocyanate component: prepare the raw materials according to Table 1 to Table 2 and mix them according to the proportion, mix them evenly to obtain the isocyanate component, and control the material temperature to 15 to 25° C.;

[0072] (2) controlling the material temperature of the polyol component to 20-30° C.;

[0073] (3) Mixing: The polyol component and the isocyanate component are mixed according to an isocyanate index of 1.05 to 1.12, and injected into a closed mold through a high-pressure foaming machine gun head at a mold temperature of 35 to 40°C. The reaction product is cured and formed to obtain a polyurethane rigid foam. The foam core density of the reaction raw materials when they are just filled in the mold, as well as the various properties of the polyurethane rigid foam obtained after overfilling by 12wt%, are measured.

[0074] The water content, hydroxyl value and viscosity are measured in accordance with the method in "HG / T 4961-2016 Polyurethane Rigid Foam Composite Polyether for Refrigerators and Freezers". The core density, dimensional stability, thermal conductivity and compressive strength are all measured in accordance with the method in "GB / T 26689-2011 Rigid Polyurethane Foam Plastics for Refrigerators and Freezers". The coefficient of variation of compressive strength is measured in accordance with the method in "GB / T35453-2017 Rigid Polyurethane Foam Board (DLPU) for Frozen Soil Roadbed". The detection method of NCO mass fraction is measured in accordance with the method in "GB / T 12009.4-2016 Aromatic Isocyanates for Plastic Polyurethane Production Part 4: Determination of Isocyanate Content". The expansion rate after 2min demoulding is the thickness change rate of the foam measured from the start of injection to 2min after demoulding (the difference between the maximum foam thickness after demoulding and the mold thickness as a percentage of the mold thickness). The shorter the demoulding time and the smaller the thickness change rate, the better the curing performance.

[0075] Example 1

[0076] According to the isocyanate index of 1.10, the S-1# isocyanate component was mixed with 115 parts of the polyol component H9506. Before mixing, the viscosity difference between the polyol component and the isocyanate component at 25°C was 168 mPa·s, and the mixing pressure was 150 bar. The polyurethane rigid foam was injected into the mold for curing and formed, and was recorded as PU-1#.

[0077] Example 2

[0078] According to the isocyanate index of 1.10, the S-2# isocyanate component was mixed with 116 parts of the polyol component H9585.3. Before mixing, the viscosity difference between the polyol component and the isocyanate component at 25°C was 24 mPa·s, the mixing pressure was 120 bar, and the polyurethane rigid foam was obtained by injection into a mold for curing and molding, and was recorded as PU-2#.

[0079] Example 3

[0080] According to the isocyanate index of 1.10, the S-3# isocyanate component was mixed with 115 parts of the polyol component H9506. Before mixing, the viscosity difference between the polyol component and the isocyanate component at 25°C was 300 mPa·s, and the mixing pressure was 160 bar. The polyurethane rigid foam was injected into the mold for curing and molding, and was recorded as PU-3#.

[0081] Example 4

[0082] The S-4# isocyanate component was mixed with 117 parts of the polyol component H9557.1 according to the isocyanate index of 1.10. The viscosity difference between the polyol component and the isocyanate component at 25°C before mixing was 2189 mPa·s. The mixing pressure was 120 bar. The polyurethane rigid foam was injected into the mold for curing and was recorded as PU-4#.

[0083] Example 5

[0084] According to the isocyanate index of 1.10, the S-5# isocyanate component was mixed with 116 parts of the polyol component H9585.3. Before mixing, the viscosity difference between the polyol component and the isocyanate component at 25°C was 424 mPa·s, and the mixing pressure was 120 bar. The polyurethane rigid foam was injected into the mold for curing and was recorded as PU-5#.

[0085] Example 6

[0086] According to the isocyanate index of 1.12, the S-6# isocyanate component was mixed with 116 parts of the polyol component H9585.3. Before mixing, the viscosity difference between the polyol component and the isocyanate component at 25°C was 150 mPa·s, and the mixing pressure was 130 bar. The polyurethane rigid foam was injected into the mold for curing and was recorded as PU-6#.

[0087] Example 7

[0088] According to the isocyanate index of 1.10, the S-7# isocyanate component was mixed with 116 parts of the polyol component H9683. Before mixing, the viscosity difference between the polyol component and the isocyanate component at 25°C was 426 mPa·s, and the mixing pressure was 130 bar. The polyurethane rigid foam was injected into the mold for curing and was recorded as PU-7#.

[0089] Example 8

[0090] The S-8# isocyanate component was mixed with 116 parts of the polyol component H9584 according to the isocyanate index of 1.10. The viscosity difference between the polyol component and the isocyanate component at 25°C before mixing was 379 mPa·s, and the mixing pressure was 160 bar. The polyurethane rigid foam was injected into the mold for curing and was recorded as PU-8#.

[0091] Example 9

[0092] According to the isocyanate index of 1.12, the S-9# isocyanate component was mixed with 115 parts of the polyol component H9537.1. Before mixing, the viscosity difference between the polyol component and the isocyanate component at 25°C was 494 mPa·s, and the mixing pressure was 160 bar. The polyurethane rigid foam was injected into the mold for curing and was recorded as PU-9#.

[0093] Example 10

[0094] According to the isocyanate index of 1.05, the S-10# isocyanate component was mixed with 115 parts of the polyol component H9537.1. Before mixing, the viscosity difference between the polyol component and the isocyanate component at 25°C was 342 mPa·s, and the mixing pressure was 120 bar. The polyurethane rigid foam was injected into the mold for curing and was recorded as PU-10#.

[0095] Embodiment 11

[0096] According to the isocyanate index of 1.12, the S-11# isocyanate component was mixed with 115 parts of the polyol component H9537.1. Before mixing, the viscosity difference between the polyol component and the isocyanate component at 25°C was 701 mPa·s, and the mixing pressure was 160 bar. The polyurethane rigid foam was injected into the mold for curing and was recorded as PU-11#.

[0097] Example 12

[0098] According to the isocyanate index of 1.10, the S-12# isocyanate component was mixed with 116 parts of the polyol component H9584. Before mixing, the viscosity difference between the polyol component and the isocyanate component at 25°C was 344 mPa·s, and the mixing pressure was 120 bar. The polyurethane rigid foam was injected into the mold for curing and was recorded as PU-12#.

[0099] Comparative Example 1

[0100] DS-1# was mixed with 116 parts of polyol component H9683 according to the isocyanate index of 1.10. The viscosity difference between the polyol component and the isocyanate component at 25°C was 343 mPa·s before mixing. The mixing pressure was 130 bar. The polyurethane rigid foam was injected into the mold for curing and was recorded as DPU-1#.

[0101] Comparative Example 2

[0102] DS-2# was mixed with 116 parts of polyol component H9585.3 according to the isocyanate index of 1.12. The viscosity difference between the polyol component and the isocyanate component at 25°C was 517 mPa·s before mixing. The mixing pressure was 120 bar. The polyurethane rigid foam was injected into the mold for curing and was recorded as DPU-2#.

[0103] Comparative Example 3

[0104] DS-3# was mixed with 116 parts of polyol component H9524 according to the isocyanate index of 1.10. The viscosity difference between the polyol component and the isocyanate component at 25°C was 159 mPa·s before mixing. The mixing pressure was 120 bar. The polyurethane rigid foam was injected into the mold for curing and was recorded as DPU-3#.

[0105] Comparative Example 4

[0106] DS-4# was mixed with 115 parts of polyol component H9506 according to the isocyanate index of 1.10. The viscosity difference between the polyol component and the isocyanate component at 25°C was 3921 mPa·s before mixing. The mixing pressure was 160 bar. The polyurethane rigid foam was injected into the mold for curing and was recorded as DPU-4#.

[0107] Comparative Example 5

[0108] DS-5# was mixed with 116 parts of polyol component H9585.3 according to the isocyanate index of 1.10. The viscosity difference between the polyol component and the isocyanate component at 25°C was 160 mPa·s before mixing. The mixing pressure was 120 bar. The polyurethane rigid foam was injected into the mold for curing and was recorded as DPU-5#.

[0109] The performance of the prepared polyurethane rigid foam was characterized, and the results are shown in Table 3 and Table 4.

[0110] Table 3 PU-1#~PU-9# polyurethane rigid foam performance characterization results

[0111]

[0112] Table 4 PU-10#~DPU-5# polyurethane rigid foam performance characterization results

[0113]

[0114]

[0115] It can be seen from the data in Table 3 and Table 4 that the technical solution of the present invention can effectively improve the thermal conductivity, and the obtained polyurethane rigid foam also has good fluidity and stability, including demoulding stability, storage stability and dimensional stability, and has good comprehensive performance.

[0116] Specifically, the modified isocyanate A of the present invention can effectively reduce the thermal conductivity of polyurethane rigid foam, especially when the modified isocyanate A is used alone or the proportion of the modified isocyanate A is high, the improvement effect on the thermal conductivity is particularly obvious. However, compared with the technical solution of modified isocyanate A and organic isocyanate blending, the demoulding deformation rate of modified isocyanate A alone is slightly higher (such as: the expansion rate after demoulding of Example 4 is the highest, and the expansion rate after demoulding of Example 5 is higher than that of Example 2), but it does not affect the use of foam. For applications with higher energy consumption requirements, the present invention may preferably use the technical solution of modified isocyanate A blended with organic isocyanate to combine thermal conductivity and demoulding stability. Further considering the various excellent properties of polyurethane rigid foam, isocyanates modified with cyclic polyols are preferred. Therefore, the present invention preferably uses Examples 1, 2, 3, 6 to 12, and most preferably 8 to 12.

[0117] In contrast, in Example 1, high-functionality polymethylene polyphenyl polyisocyanate is used as the isocyanate component, and no modified isocyanate A is used. The improvement effect on the thermal conductivity of the polyurethane rigid foam is poor. In Example 2, modified isocyanate A with a NCO reduction of more than 73% is used, and a mass ratio of 1:9 is used together with polymethylene polyphenyl polyisocyanate as the isocyanate component. The thermal conductivity of the obtained rigid foam is still relatively high, and since the NCO reduction of the modified isocyanate A is relatively high, the compression strength distribution coefficient and demolding stability are further affected. In Example 3, a hydroxyl value of less than 330 mgKOH / g and a functional The polyol component with a degree of NCO less than 2.5 reacts with the isocyanate component of the present invention, and the thermal conductivity of the obtained rigid polyurethane foam is slightly improved, but the compressive strength and dimensional stability are poor; Comparative Example 4 uses only modified isocyanate A with an NCO% of 13% as the isocyanate component, resulting in low overall NCO% and functionality of the modified isocyanate component, and the performance of the obtained polyurethane rigid foam is extremely poor; Comparative Example 5 uses modified isocyanate A with an NCO reduction of less than 9%, and uses it together with polymethylene polyphenyl polyisocyanate at a mass ratio of 1:9 as the isocyanate component, and the performance improvement effect of the obtained rigid foam is not obvious.

[0118] As described above, although the present invention has been shown and described with reference to specific preferred embodiments, it should not be construed as limiting the present invention itself. Various changes in form and details may be made without departing from the spirit and scope of the present invention as defined in the appended claims.

Claims

1. A method for preparing a polyurethane rigid foam, characterized in that: The polyol component and the isocyanate component are mixed and reacted to obtain the polyurethane rigid foam; the polyol component contains polyether polyol and / or polyester polyol, a foaming agent, a foam stabilizer and a catalyst; the isocyanate component contains modified isocyanate A, the modified isocyanate A is an organic isocyanate modified by a hydroxyl compound, the organic isocyanate is at least one of diphenylmethane diisocyanate, toluene diisocyanate or polymethylene polyphenyl polyisocyanate, the NCO% of the organic isocyanate is N1, the NCO% of the modified isocyanate A is N2, (1-N2 / N1)×100%≤73%; based on the total mass of the isocyanate component, the mass proportion of the modified isocyanate A is ≥5%; the average hydroxyl value of the polyol component when not containing a foaming agent is 330-480 mgKOH / g, and the average functionality is ≥3.5; the NCO% of the isocyanate component is 17.0-31.3%, and the average functionality is ≥2.

2.

2. The preparation method according to claim 1, characterized in that: The modified isocyanate A is an organic isocyanate modified by a hydroxy compound containing a ring-containing polyol.

3. The preparation method according to claim 2, characterized in that: The isocyanate component is composed of modified isocyanate A and polymethylene polyphenyl polyisocyanate, or is composed of modified isocyanate A, polymethylene polyphenyl polyisocyanate and an inert auxiliary agent; wherein, based on the total mass of the isocyanate component, the mass proportion of modified isocyanate A is ≤25%.

4. The preparation method according to claim 1, characterized in that: The viscosity of the isocyanate component at 25° C. is greater than 500 mPa·s.

5. The preparation method according to claim 4, characterized in that: The viscosity difference between the polyol component and the isocyanate component at 25° C. is ≤700 mPa·s.

6. The preparation method according to claim 4, characterized in that: The pressure when the polyol component and the isocyanate component are mixed is 120-160 bar.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The foaming agent contains an alkane compound.

8. The preparation method according to any one of claims 1 to 6, characterized in that: The average functionality of the polyol component is 3.5 to 5.

0.

9. The preparation method according to claim 8, characterized in that: The average hydroxyl value of the polyol component when not containing a blowing agent is 350 to 460 mgKOH / g.

10. An isocyanate component, characterized in that The isocyanate component contains modified isocyanate A, and the modified isocyanate A is an organic isocyanate modified by a hydroxyl compound. The organic isocyanate is at least one of diphenylmethane diisocyanate, toluene diisocyanate or polymethylene polyphenyl polyisocyanate. The NCO% of the organic isocyanate is N1, and the NCO% of the modified isocyanate A is N2. (1-N2 / N1)×100%≤73%. Based on the total mass of the isocyanate component, the mass proportion of the modified isocyanate A is ≥5%, the NCO% of the isocyanate component is 17.0-31.3%, and the average functionality is ≥2.2.