Method for preparing liquid regenerated rubber at low temperature through two-time desulfurization and liquid regenerated rubber

Through two desulfurization and low temperature preparation methods, the problems of high energy consumption and low added value of traditional recycled rubber are solved, a low-carbon and environmentally friendly production process is achieved, and the mechanical properties and resource utilization efficiency of rubber are improved.

CN118909336APending Publication Date: 2024-11-08JIANGSU LVJINREN TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411188377.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The production of traditional recycled rubber has problems such as high energy consumption, high pollution and low added value, and there are serious safety hazards and energy consumption during the desulfurization process, and the mechanical properties of recycled rubber are not compatible with downstream doping.

Method used

The method of preparing liquid regenerated rubber by preheating the waste rubber powder with activator and desulfurization is performed once in the screw extruder, and then mixing it with the softener and performing a second desulfurization under low temperature conditions. Cooling and forming, the geometric arrangement of the screw extruder isolates oxygen, and achieves a high shear and low temperature desulfurization process.

Benefits of technology

Reduces the decomposition of rubber hydrocarbons and additives, improves the molecular weight and viscosity of hydrocarbon polymer chains of liquid regenerated rubber, reduces production energy consumption, increases the added value of resource utilization, and enhances the use of raw rubber, carbon black, and operation. Compatibility between oil and resin, stable and controllable production process, low-carbon and environmentally friendly.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a method for preparing liquid regenerated rubber at low temperature through twice desulfurization and liquid regenerated rubber liquid, and the method comprises the following steps: mixing and preheating waste rubber powder and desulfurizer raw materials, conveying into a first screw extruder, heating and preliminarily desulfurizing, conveying into a mixing device, and mixing with a softener to further reduce the viscosity, so as to obtain the liquid regenerated rubber. And feeding into a second screw extruder, continuously extruding under the action of high shear, and cooling and molding to obtain the liquid regenerated rubber. The two desulfurization processes not only realize the existence of oxygen isolation, but also reduce the decomposition of rubber hydrocarbon and auxiliaries compared with the traditional high-temperature preparation of liquid regenerated rubber, the efficiency is high, the process is continuous and automatic, the labor is saved, and the production process is stable and controllable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of chemical materials, and in particular to a method for preparing liquid regenerated rubber by double desulfurization at low temperature and the liquid regenerated rubber. Background Art

[0002] Recycled rubber has become the third most widely used type of rubber after natural rubber and synthetic rubber. The reclaimed rubber industry has formed a desulfurization and regeneration process based on "dynamic desulfurization at high temperature and high pressure". The desulfurization reaction is completed in the desulfurization tank. The regeneration agent and water are added to the desulfurization tank together. The working pressure is about 2.2MPa and the working temperature is about 220℃. After the desulfurization time is about 2 hours, the material is taken out after pressure relief and cooling to obtain desulfurized rubber powder, and then it is pressed into sheets by 3 to 4 high-speed refining machines to obtain reclaimed rubber. The penetration of the regeneration agent into the waste rubber is completed at high temperature and high pressure for a long time, which poses serious safety hazards and consumes a lot of energy. The desulfurized rubber powder needs to be cooled from the high temperature state to room temperature by the outside world, and the refining process requires continuous low temperature, resulting in a large amount of energy consumption. When recycled rubber is added to tire products, it partially replaces raw rubber, carbon black, operating oil and resin, etc., which is not closely related to the mechanical properties of the recycled rubber itself. It pays more attention to the effective content and stability of each component of recycled rubber, and does not blindly pursue the physical properties in GB / T 13460-2016 "Recycled Rubber". At present, most manufacturers in the industry are still oriented to the pursuit of high-strength recycled rubber, which is obviously out of touch with downstream mixing, which also leads to the problems of high energy consumption, high pollution and low added value in traditional recycled rubber production, which are difficult to solve.

[0003] In recent years, the industry has been actively promoting the high-value recycling of waste rubber, such as returning rubber, liquid, low-viscosity recycled rubber and other new products are emerging. Zhang Liqun et al. selected a rubber powder particle size of 0.1-10mm in CN102601975B "A method for continuously preparing liquid recycled rubber using a screw extruder", believing that the required recycled rubber can be obtained by extruding the material from the screw head, without the need for subsequent refining and other processes, which greatly reduces energy consumption; but did not realize the inevitable "half-cooked" situation in the process of rubber powder desulfurization. The Mooney viscosity ML100℃1+4 of the recycled rubber particles prepared by Zhang Jianwu et al. in CN201910308916.6 "A low Mooney viscosity recycled rubber particle and its preparation method and use" is 15-40, and the sol content is greater than 30%. It is used for waterproof membranes or road construction, and the fineness of the liquid glue is not required. The particle size is 10-80 mesh, and the rubber powder is preheated at high temperature using a high-speed mixer, and then discharged into a kneading machine for kneading and mixing and cooled to below 160°C; then discharged through a screw extruder for mixing, and further granulated through a die head water pelletizer to obtain low Mooney viscosity recycled rubber particles. Under such high temperature conditions, the rubber powder is inevitably subject to thermal oxidation aging.

[0004] How to better protect the original effective ingredients in waste rubber such as rubber hydrocarbons, carbon black and resin, and reduce the problem of uneven "core-shell" structure in desulfurization and regeneration, cannot blindly follow the experience of traditional recycled rubber, but requires new solutions between equipment, formula and process from the new product itself. Therefore, this application designs the scheme in principle under the new demand, prepares a new type of liquid recycled rubber to fully replace the role of raw rubber, carbon black, operating oil and resin, and improves the added value of recycled rubber for resource utilization. Summary of the invention

[0005] The present invention provides a method for preparing liquid regenerated rubber by double desulfurization at low temperature and liquid regenerated rubber, so as to solve or at least alleviate at least one problem existing in the prior art.

[0006] The present invention provides a method for preparing liquid regenerated rubber by double desulfurization at low temperature, the method comprising:

[0007] 100 parts of waste rubber powder and 0 to 5 parts of activator are uniformly preheated and mixed by weight; the activator comprises a compound of two or more of aromatic disulfide, polyalkylphenol sulfide, phenyl mercaptan and amino compound;

[0008] The uniformly preheated and mixed raw materials are fed into a first screw extruder to extrude the devulcanized rubber;

[0009] 100 parts of the desulfurized rubber and 0 to 10 parts of a softener are continuously transferred into a mixing device for continuous mixing, based on parts by mass; the activator comprises a compound of two or more of environmentally friendly aromatic oil, pine tar, tall oil, naphthenic oil, dipentene, paraffin oil, oleic acid, and rosin;

[0010] The mixed rubber is sent to a second screw extruder for extrusion, and liquid recycled rubber is obtained after cooling and molding.

[0011] As a preferred embodiment of the present invention, the particle size of the waste rubber powder is 18 to 40 meshes; the waste rubber powder is obtained by crushing waste rubber tires and removing impurities; the waste rubber tires include one or more of all-steel load-bearing tires, passenger car tires, bias load-bearing tires and light truck tires.

[0012] As a preferred embodiment of the present invention, the uniformly preheating and mixing of 100 parts of waste rubber powder and 0 to 5 parts of activator comprises:

[0013] Preheat and mix 100 parts of waste rubber powder and 0-5 parts of activator uniformly at 80-120°C under the action of a stirring device within 5-20 minutes.

[0014] As a preferred embodiment of the present invention, the first screw extruder includes a single screw, a twin screw or a multi-screw; the aspect ratio of the first screw extruder is (28-48):1, and the threaded element consists of a conveying element and a shearing element.

[0015] As a preferred embodiment of the present invention, the process of feeding the uniformly preheated and mixed raw materials into a first screw extruder for extrusion to obtain devulcanized rubber comprises:

[0016] The uniformly preheated and mixed raw materials are fed into a first screw extruder, wherein the temperature of the heating section of the first screw extruder is controlled at 120°C to 180°C, the temperature of the mixing section is controlled at 180°C to 220°C, the temperature of the insulation section is controlled at 120°C to 180°C, and the reaction is carried out for 1 to 10 minutes before extrusion to obtain devulcanized rubber.

[0017] As a preferred embodiment of the present invention, the mixing device comprises a high-speed refiner or a screw extruder, and the mixing temperature of the mixing device is controlled at 20-80°C.

[0018] As a preferred embodiment of the present invention, the screw extruder is a twin-screw or multi-screw extruder.

[0019] As a preferred embodiment of the present invention, the second screw extruder includes a twin-screw extruder or a multi-screw extruder; the aspect ratio of the second screw extruder is (32-48):1.

[0020] As a preferred embodiment of the present invention, the mixed rubber is fed into a second screw extruder for extrusion, and the liquid regenerated rubber is obtained after cooling and molding, comprising:

[0021] The mixed rubber is sent to a second screw extruder, the temperature of the heating section of the second screw extruder is controlled at 80°C to 120°C, the temperature of the mixing section is controlled at 120°C to 200°C, the temperature of the insulation section is controlled at 80 to 120°C, and the reaction is carried out for 2 to 5 minutes before extrusion. After cooling and molding, liquid regenerated rubber is obtained to obtain devulcanized rubber.

[0022] The present invention provides a liquid regenerated rubber, which is prepared by the method for preparing liquid regenerated rubber by double desulfurization at low temperature as claimed in any one of claims 1 to 9.

[0023] Compared with the prior art, the present invention has at least the following beneficial effects:

[0024] After analyzing the downstream applications of traditional "solid" recycled rubber, we know that there are problems that need to be solved when "solid" rubber is used as a filler in products: (1) fineness problem. The root cause is the poor thermal conductivity of rubber, and the slow heat transfer during the desulfurization process causes poor uniformity; (2) the necessary conditions for the original components to be effectively utilized after the desulfurization process: avoid high temperature decomposition and oxygen oxidation; be able to be fully released from the original cross-linked network. Under the conditions of low temperature, oxygen isolation and high shear, a process configuration of mixed preheating, primary desulfurization and mixing, secondary desulfurization and cooling molding was designed: in the preheating and mixing process, the waste rubber is devolatile at a temperature lower than the strong oxidation temperature and the preheating temperature is increased as much as possible on the basis of uniform mixing. After the waste rubber is initially desulfurized at a low temperature, the destruction of rubber hydrocarbons is minimized. After the cross-linking network is partially destroyed, it is mixed with a softener. The softener can more easily penetrate and evenly enter the interior of the waste rubber powder. The mixing process also further reduces the viscosity of the desulfurized rubber, so that the second desulfurization regeneration conditions can be milder. Under relatively low temperature conditions, the original carbon black and additives are fully released under high shear to obtain liquid recycled rubber.

[0025] Taking advantage of the flexible and changeable geometric arrangement of the screw extruder, the softener and activator are added at different positions. The two desulfurization processes not only isolate the presence of oxygen, but also reduce the decomposition of rubber hydrocarbons and additives compared to the previous high-temperature preparation of liquid recycled rubber. The tandem screw extruder unit has a short time, high efficiency, and a continuous and automated process, which saves labor and makes the production process stable and controllable.

[0026] The prepared liquid recycled rubber hydrocarbon polymer chain has a high molecular weight, little damage to the original additives in the waste rubber, and low viscosity. When used downstream, it can replace more raw rubber, carbon black, operating oil and resin, etc. Compared with the addition of traditional recycled rubber, it has better processing performance, smoother product surface, low-carbon and environmentally friendly production process, which greatly increases the added value of waste rubber resource utilization. DETAILED DESCRIPTION

[0027] Exemplary embodiments of the present invention will be described in more detail below. The present invention provides exemplary embodiments, but it should be appreciated that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to be able to more thoroughly understand the present invention, and the scope of the present invention can be fully communicated to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0028] Example 1

[0029] 100 parts of 18-mesh waste passenger tire rubber powder and 2 parts of activator aromatic disulfide are stirred for 20 minutes to reach 120°C, and then added to a single screw extruder with a length-to-diameter ratio of 48:1 of a first screw extruder, the temperature of the heating section is controlled at 180°C, the temperature of the mixing section is controlled at 220°C, the temperature of the insulation section is controlled at 180°C, and the desulfurized rubber is extruded after reacting for 10 minutes. The desulfurized rubber is added to 8 parts of aromatic oil in two high-speed refiners and mixed evenly at 20°C, and then sent to a second twin-screw extruder with a length-to-diameter ratio of 32:1, the temperature of the heating section is controlled at 80°C, the temperature of the mixing section is controlled at 150°C, the temperature of the insulation section is controlled at 80°C, and the reaction is carried out for 2 minutes. The liquid regenerated rubber is obtained after cooling and molding to obtain the desulfurized rubber.

[0030] Example 2

[0031] 100 parts of 22-mesh all-steel truck tire rubber powder and 5 parts of polyalkylphenol sulfide activator are stirred for 5 minutes to reach 100°C, and then added to a twin-screw extruder with a length-to-diameter ratio of 32:1 of a first screw extruder, the temperature of the heating section is controlled at 150°C, the temperature of the mixing section is controlled at 200°C, the temperature of the insulation section is controlled at 150°C, and the desulfurized rubber is extruded after reacting for 5 minutes. The desulfurized rubber is added to a second twin-screw extruder and mixed evenly at 50°C, and then sent to a third twin-screw extruder with a length-to-diameter ratio of 40:1, the temperature of the heating section is controlled at 120°C, the temperature of the mixing section is controlled at 200°C, the temperature of the insulation section is controlled at 120°C, and the reaction is carried out for 3 minutes. The desulfurized rubber is obtained after cooling and molding.

[0032] Example 3

[0033] 100 parts of 40-mesh all-steel truck tire rubber powder were stirred for 10 minutes to reach 80°C, and then added to a parallel three-screw extruder with a length-to-diameter ratio of 28:1 of the first screw extruder. The temperature of the heating section was controlled at 120°C, the temperature of the mixing section was controlled at 180°C, and the temperature of the insulation section was controlled at 120°C. After reaction for 1 minute, the desulfurized rubber was extruded, added to a second twin-screw extruder and mixed evenly with 5 parts of paraffin oil at 80°C, and then sent to a third twin-screw extruder with a length-to-diameter ratio of 48:1. The temperature of the heating section was controlled at 90°C, the temperature of the mixing section was controlled at 160°C, and the temperature of the insulation section was controlled at 90°C. After reaction for 5 minutes, the desulfurized rubber was extruded, and liquid recycled rubber was obtained after cooling and molding to obtain desulfurized rubber.

[0034] The various properties of the liquid recycled rubber prepared in Examples 1 to 3 are shown in the following table.

[0035] project Example 1 Example 2 Example 3 Heating loss, % 1.0 1.0 1.0 Sol content, % 73 81 85 Sol molecular weight Mn 11362 9530 13234 <![CDATA[Density g·cm -3 > 1.19 1.17 1.15

Claims

1. A method for preparing liquid regenerated rubber by double desulfurization at low temperature, characterized in that: The method includes: 100 parts of waste rubber powder and 0 to 5 parts of activator are uniformly preheated and mixed by weight; the activator comprises a compound of two or more of aromatic disulfide, polyalkylphenol sulfide, phenyl mercaptan and amino compound; The uniformly preheated and mixed raw materials are fed into a first screw extruder to extrude the devulcanized rubber; 100 parts of the desulfurized rubber and 0 to 10 parts of a softener are continuously transferred into a mixing device for continuous mixing, based on parts by mass; the activator comprises a compound of two or more of environmentally friendly aromatic oil, pine tar, tall oil, naphthenic oil, dipentene, paraffin oil, oleic acid, and rosin; The mixed rubber is sent to a second screw extruder for extrusion, and liquid recycled rubber is obtained after cooling and molding.

2. The method for preparing liquid regenerated rubber by double desulfurization at low temperature according to claim 1, characterized in that: The particle size of the waste rubber powder is 18-40 meshes; the waste rubber powder is obtained by crushing waste rubber tires and removing impurities; the waste rubber tires include one or more of all-steel load-bearing tires, passenger car tires, bias load-bearing tires and light truck tires.

3. The method for preparing liquid regenerated rubber by double desulfurization at low temperature according to claim 1, characterized in that: The method of uniformly preheating and mixing 100 parts of waste rubber powder and 0 to 5 parts of activator comprises: Preheat and mix 100 parts of waste rubber powder and 0-5 parts of activator uniformly at 80-120°C under the action of a stirring device within 5-20 minutes.

4. The method for preparing liquid regenerated rubber by double desulfurization at low temperature according to claim 1, characterized in that: The first screw extruder includes a single screw, a twin screw or a multi-screw; the length-to-diameter ratio of the first screw extruder is (28-48):1, and the threaded element is composed of a conveying element and a shearing element.

5. The method for preparing liquid regenerated rubber by double desulfurization at low temperature according to claim 5, characterized in that: The process of feeding the uniformly preheated and mixed raw materials into a first screw extruder to extrude the devulcanized rubber comprises: The uniformly preheated and mixed raw materials are fed into a first screw extruder, wherein the temperature of the heating section of the first screw extruder is controlled at 120°C to 180°C, the temperature of the mixing section is controlled at 180°C to 220°C, the temperature of the insulation section is controlled at 120°C to 180°C, and the reaction is carried out for 1 to 10 minutes before extrusion to obtain devulcanized rubber.

6. The method for preparing liquid regenerated rubber by double desulfurization at low temperature according to claim 1, characterized in that: The mixing device comprises a high-speed refiner or a screw extruder, and the mixing temperature of the mixing device is controlled at 20-80°C.

7. The method for preparing liquid regenerated rubber by double desulfurization at low temperature according to claim 6, characterized in that: The screw extruder is a twin-screw or multi-screw extruder.

8. The method for preparing liquid regenerated rubber by double desulfurization at low temperature according to claim 1, characterized in that: The second screw extruder includes a twin-screw extruder or a multi-screw extruder; the aspect ratio of the second screw extruder is (32-48):

1.

9. The method for preparing liquid regenerated rubber by double desulfurization at low temperature according to claim 8, characterized in that: The mixed rubber is sent to a second screw extruder for extrusion, and the liquid regenerated rubber is obtained after cooling and molding, comprising: The mixed rubber is sent to a second screw extruder, the temperature of the heating section of the second screw extruder is controlled at 80°C to 120°C, the temperature of the mixing section is controlled at 120°C to 200°C, the temperature of the insulation section is controlled at 80 to 120°C, and the reaction is carried out for 2 to 5 minutes before extrusion. After cooling and molding, liquid regenerated rubber is obtained to obtain devulcanized rubber.

10. A liquid recycled rubber, characterized in that: The liquid regenerated rubber is prepared by the method for preparing liquid regenerated rubber by double desulfurization at low temperature as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for continuously preparing liquid reclaimed rubber by aid of screw extruder

    CN102601975A

  • Method for preparing reclaimed rubber by continuous low-temperature high shear

    CN102816343A

  • Method for continuous preparation of reclaimed rubber by using dual-band twin-screw extruder

    CN102977404A

  • Method for preparation of reclaimed rubber by multi-stage screw continuous desulfurization

    CN107936331A