Preparation method of environment-friendly aluminum passivation film-forming agent

Through the preparation method of environmentally friendly aluminum passivation film forming agent and the treatment of blower drying box, the problems of chromium pollution and low efficiency in aluminum passivation are solved, efficient decontamination, corrosion resistance and mechanical properties are achieved, and rapid and uniform drying is achieved. , improve product quality.

CN118910602APending Publication Date: 2024-11-08ANHUI HUAYAO NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410986015.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The use of high-concentration chromate solution in the existing aluminum passivation technology causes hexavalent chromium contamination, posing a threat to ring and human health, and has low manual cleaning efficiency, affecting the passivation effect.

Method used

The preparation method of environmentally friendly aluminum passivation film forming agent is adopted, including degreasing cleaning, pickling, neutralization, hot water washing, activation, water washing, passivation and drying, and sodium nitrite, chromium nitrate, organic acid complexing agent, etc. The passivation liquid of the components is dried in combination with a blower drying box.

Benefits of technology

Effectively remove oil stains and oxides, improve the finish and corrosion resistance of aluminum surface, form a dense oxide film, enhance hardness and wear resistance, improve mechanical properties, and quickly and evenly dry through a blow drying box, reduce moisture risks, and improve product Quality and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910602A_ABST
    Figure CN118910602A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an environment-friendly aluminum passivation film-forming agent, which relates to the technical field of metal surface treatment and comprises the following steps of degreasing cleaning, acid pickling, hot water washing, activation, water washing, passivation, water washing, hot water washing and drying. In the drying process, an air blast drying box is further included, a pair of symmetrically-distributed side plates are fixedly arranged on the inner bottom wall of the air blast drying box, a carrying plate is arranged on the outer side of each side plate, a plurality of carrying grooves distributed at equal intervals are formed in the top face of each carrying plate, and a plurality of evenly-distributed leakage holes are formed in the inner bottom wall of each carrying groove. And die-casting aluminum is placed in each object carrying groove. After the die-casting aluminum is subjected to passivation treatment, impurities such as oil stains and oxides can be removed, a layer of compact oxidation film is formed on the surface of the die-casting aluminum under the action of the passivation layer, and the oxidation film has certain hardness and wear resistance, so that the hardness and wear resistance of the surface of the die-casting aluminum can be enhanced, and the mechanical property of the die-casting aluminum is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal surface treatment, and in particular to a method for preparing an environmentally friendly aluminum passivation film-forming agent. Background Art

[0002] During the production and use of die-cast aluminum, passivation treatment is often required to remove impurities such as oil, oxides, etc., and to improve the surface cleanliness and corrosion resistance of die-cast aluminum.

[0003] As disclosed in the Chinese invention patent, the passivation solution for trivalent chromium passivation of high silicon die-cast aluminum alloy (publication number: CN113584469B) includes: chromium nitrate 3-10g / L, organic acid complexing agent 2-8g / L, polyhydroxy alcohol complexing agent 1-6g / L, corrosion resist 1-3g / L, film-forming promoter 1-3g / L, and the passivation process is degreasing and degreasing-hot water washing-activation-water washing-passivation-water washing-hot water washing-drying.

[0004] After die-cast aluminum is formed, the surface of the die-cast aluminum is usually passivated. Generally, a high-concentration or medium-concentration chromate solution is used to passivate the coating to improve the corrosion resistance of the coating. However, hexavalent chromium pollution produced by chromate causes serious harm to the environment and human health, and manual cleaning is inefficient, which affects the passivation effect. Summary of the invention

[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a method for preparing an environmentally friendly aluminum passivation film-forming agent.

[0006] In order to solve the problems existing in the prior art, the present invention adopts the following technical solutions:

[0007] A method for preparing an environmentally friendly aluminum passivation film-forming agent comprises the following steps:

[0008] S1. Degreasing and cleaning: Soak the die-cast aluminum in degreasing liquid for 20-40 minutes. Keep the degreasing liquid at a temperature of 60-80°C to ensure that the oil and impurities are completely removed. Remove the oil, dust and other impurities on the surface of the die-cast aluminum;

[0009] The degreasing liquid includes 8-10% sodium hydroxide, 1.5-2.5% sodium carbonate, 4% sodium phosphate, 2% sodium silicate, and water. The degreasing liquid uses the wettability, permeability, emulsification and dispersibility of the surfactant to remove dirt from the surface of the die-cast aluminum.

[0010] S2. Pickling: Immerse the die-cast aluminum in a pickling solution to remove the oxide scale and oxide layer on the surface of the die-cast aluminum and improve the surface finish to prepare for passivation treatment. The pickling solution includes 15% hydrochloric acid, 1% hexamethylenetetramine, 3% hydrofluoric acid, 10% nitric acid, and water;

[0011] After pickling, the die-cast aluminum is neutralized with a neutralizing solution, which includes 2% ammonia water and water. The die-cast aluminum is fully rinsed with flowing neutralizing solution to remove residual pickling solution and other chemicals to ensure that the surface of the die-cast aluminum is no longer acidic.

[0012] S3. Hot water washing: Wash the die-cast aluminum with hot water at a temperature of 60-80℃ for 30-40s to ensure that the die-cast aluminum is thoroughly cleaned and avoid the residual pickling liquid from affecting the subsequent use of the die-cast aluminum;

[0013] S4. Activation: At room temperature, use 5-10 ml / L of hydrofluoric acid to activate the die-cast aluminum for 20-30 seconds;

[0014] S5. Water washing: Wash the die-cast aluminum with deionized water for 30-40 seconds at room temperature to prevent activation residues from affecting the subsequent use of the die-cast aluminum.

[0015] S6. Passivation: Soak the die-cast aluminum in the passivation solution for 2-4 minutes for passivation treatment. The die-cast aluminum forms a protective passivation film to improve the corrosion resistance of the die-cast aluminum.

[0016] The passivation solution includes 10-12% sodium nitrite, 3-10% chromium nitrate, 2-8% organic acid complexing agent, 1-6% polyhydroxy alcohol complexing agent, 1-3% corrosion inhibitor, 1-3% film-forming accelerator, and water;

[0017] S7, water washing: at room temperature, the die-cast aluminum is washed with deionized water for 30-40 seconds, and the die-cast aluminum is cleaned with running water to remove the passivation liquid residue;

[0018] S8. Hot water washing: Wash the die-cast aluminum with hot water at a temperature of 60-80℃ for 30-40s to ensure that the die-cast aluminum is thoroughly cleaned to avoid the residual passivation liquid affecting the subsequent use of the die-cast aluminum;

[0019] S9, Drying: Place the passivated die-cast aluminum in a blast drying oven, keep the drying temperature in the range of 80-90°C, and dry for 5-10 minutes to avoid water marks and spots on the surface of the die-cast aluminum and ensure surface smoothness;

[0020] In step S9, a pair of rectangular openings are provided at the bottom of both side walls of the blast drying oven, each of the rectangular openings is provided with a movable hinged side door panel inside, a pair of symmetrically distributed side panels are fixedly provided on the inner bottom wall of the blast drying oven, a loading plate is provided on the outer side of each of the side panels, a plurality of equally distributed loading slots are provided on the top surface of each of the loading plates, a plurality of evenly distributed leakage holes are provided on the inner bottom wall of each of the loading slots, and die-cast aluminum is placed inside each of the loading slots.

[0021] Preferably, the degreasing liquid comprises 9% sodium hydroxide, 2% sodium carbonate, 4% sodium phosphate, 2% sodium silicate and water.

[0022] Preferably, the passivation solution comprises 11% sodium nitrite, 6.5% chromium nitrate, 5.5% organic acid complexing agent, 3.5% polyhydroxy alcohol complexing agent, 2% corrosion inhibitor, 2% film-forming accelerator and water.

[0023] Preferably, a pair of first connecting shafts are fixedly provided at the two corners at the top of the side panel, and a vertically distributed fixed swing arm is fixedly provided at the outer end of each of the first connecting shafts. A pair of penetrating second connecting shafts are hingedly inserted at the front and rear sides of the loading plate, and the inner end of each of the second connecting shafts is fixedly connected to the bottom end of the corresponding fixed swing arm.

[0024] Preferably, a pair of symmetrically distributed extended ear seats are fixedly provided on the inner bottom wall of the blast drying box, and the pair of extended ear seats are located between a pair of side panels, and a linkage shaft distributed through the top end of each of the extended ear seats is rotatably inserted, and an active swing arm is fixedly provided on the outer end of each of the linkage shafts.

[0025] Preferably, a suspended T-shaped swing arm is provided between the extended ear seat and the side plate on the same side, the top end of the active swing arm is movably hinged to the top end of the T-shaped swing arm, and a driven swing arm is fixed to the inner end of each of the first connecting shafts, and the two ends of the T-shaped swing arm are movably hinged to the top ends of a pair of driven swing arms.

[0026] Preferably, the inner end portion of each of the linkage shafts is sleeved with a concentrically fixed driven bevel gear, a laterally distributed connecting plate is fixed between the middle and upper parts of a pair of the extended ear seats, an intermittent shaft distributed through the middle of the connecting plate is rotatably inserted, and the top end of the intermittent shaft is sleeved with a concentrically fixed active bevel gear, and the active bevel gear is respectively meshed and connected with a pair of driven bevel gears.

[0027] Preferably, a transversely distributed T-shaped plate is fixedly disposed between the middle and lower parts of a pair of the elongated ear seats, a circular through hole is provided at the front end of the T-shaped plate, a servo motor with an output end facing upward is fixedly disposed inside the circular through hole, a limit cam is fixedly disposed at the motor shaft end of the servo motor, a triangular notch is provided at the front end of the limit cam, and a vertically distributed limit pin is fixedly disposed at the front end of the triangular notch;

[0028] The bottom end of the intermittent shaft is sleeved with a concentrically fixed intermittent disk, a plurality of evenly distributed arcuate notches are provided on the outer surface of the intermittent disk, a U-shaped notch is provided between an adjacent pair of arcuate notches, the top surface of the triangular notch slides against the bottom surface of the intermittent disk, the outer ring surface of the limit cam slides against the arcuate notch, and the top end of the limit pin shaft slides against the corresponding U-shaped notch and drives the intermittent disk to rotate.

[0029] Preferably, fixed rings are fixedly provided at the four corners of the top surface of the blast drying box, a drying fan with an output wind direction is fixedly provided inside each of the fixed rings, a pair of fan control modules are fixedly provided on both sides of the top surface of the blast drying box, the fan control modules are electrically connected to the adjacent pair of drying fans, and return pipes are fixedly provided at the bottom corners of the front and rear side surfaces of the blast drying box, and the top end of each of the return pipes is bent downward and faces the top port of the corresponding fixed ring.

[0030] Preferably, a pair of symmetrically distributed heating control modules are fixed on the top of the two side walls of the blast drying box, and a pair of symmetrically distributed continuous S-shaped heating wires are fixed on the top of the two side walls inside the blast drying box, and both ends of the continuous S-shaped heating wires pass through the side walls of the blast drying box and extend to the outside, and both ends of the heating control module are electrically connected to both ends of the adjacent continuous S-shaped heating wires.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. In the present invention, after the die-cast aluminum is passivated, impurities such as oil stains and oxides can be removed, the surface finish and corrosion resistance of the die-cast aluminum can be improved, and the corrosion resistance and mechanical properties of the die-cast aluminum can be improved;

[0033] 2. In the present invention, under the action of the passivation layer, a dense oxide film is formed on the surface of the die-cast aluminum. The oxide film has a certain hardness and wear resistance, which can enhance the hardness and wear resistance of the die-cast aluminum surface and improve the mechanical properties of the die-cast aluminum.

[0034] 3. In the present invention, the die-cast aluminum after passivation is dried by a blast drying oven, which uses strong wind flow to accelerate the evaporation of water. Compared with the traditional drying method, the drying process can be completed more quickly and the processing time can be reduced;

[0035] The blast drying oven can provide uniform airflow on the surface of die-cast aluminum, ensuring the consistency of the drying effect and avoiding incomplete local drying. It can effectively reduce moisture during the drying process and reduce the risk of oxidation on the surface of die-cast aluminum.

[0036] Uniform and rapid drying can reduce surface defects of die-cast aluminum, improve the appearance and performance of the final product, and ensure that it meets quality standards;

[0037] In conclusion, the blast drying oven can significantly improve the drying efficiency, uniformity and product quality during the drying process of die-cast aluminum after passivation. The efficient drying process reduces the time required for drying, thereby saving energy and production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0039] Figure 1 The present invention is a die-cast aluminum passivation treatment process flow chart;

[0040] Figure 2 It is a schematic diagram of the structure of the blast drying oven of the present invention;

[0041] Figure 3 It is a schematic cross-sectional view of the structure of the blast drying oven of the present invention;

[0042] Figure 4 It is a schematic diagram of the cross-section explosion of the blast drying box structure of the present invention;

[0043] Figure 5 It is an exploded schematic diagram of a pair of side plates and a pair of loading plates of the present invention;

[0044] Serial numbers in the figure: 1. Blast drying box; 2. Reflux pipe; 3. Side door panel; 4. Drying fan; 5. Fixed ring; 6. Fan control module; 7. Heating control module; 8. Continuous S-type heating wire; 9. Carrying plate; 10. Fixed swing arm; 11. Driven bevel gear; 12. Active swing arm; 13. Extended ear seat; 14. T-type swing arm; 15. Driven swing arm; 16. Side panel; 17. Active bevel gear; 18. Connecting plate; 19. Intermittent disk; 20. Limit cam; 21. T-type plate; 22. Servo motor; 23. Die-cast aluminum. DETAILED DESCRIPTION

[0045] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0046] Example 1: This example provides a method for preparing an environmentally friendly aluminum passivation film-forming agent. Figure 1 , including the following steps:

[0047] S1. Degreasing and cleaning: Soak the die-cast aluminum in degreasing liquid for 20-40 minutes. Keep the degreasing liquid at a temperature of 60-80°C to ensure that the oil and impurities are completely removed. Remove the oil, dust and other impurities on the surface of the die-cast aluminum;

[0048] The degreasing liquid includes 8-10% sodium hydroxide, 1.5-2.5% sodium carbonate, 4% sodium phosphate, 2% sodium silicate, and water. The degreasing liquid uses the wettability, permeability, emulsification and dispersibility of the surfactant to remove dirt from the surface of the die-cast aluminum.

[0049] S2. Pickling: Immerse the die-cast aluminum in a pickling solution to remove the oxide scale and oxide layer on the surface of the die-cast aluminum and improve the surface finish to prepare for passivation treatment. The pickling solution includes 15% hydrochloric acid, 1% hexamethylenetetramine, 3% hydrofluoric acid, 10% nitric acid, and water;

[0050] After pickling, the die-cast aluminum is neutralized with a neutralizing solution, which includes 2% ammonia water and water. The die-cast aluminum is fully rinsed with flowing neutralizing solution to remove residual pickling solution and other chemicals to ensure that the surface of the die-cast aluminum is no longer acidic.

[0051] S3. Hot water washing: Wash the die-cast aluminum with hot water at a temperature of 60-80℃ for 30-40s to ensure that the die-cast aluminum is thoroughly cleaned and avoid the residual pickling liquid from affecting the subsequent use of the die-cast aluminum;

[0052] S4. Activation: At room temperature, use 5-10 ml / L of hydrofluoric acid to activate the die-cast aluminum for 20-30 seconds;

[0053] S5. Water washing: Wash the die-cast aluminum with deionized water for 30-40 seconds at room temperature to prevent activation residues from affecting the subsequent use of the die-cast aluminum.

[0054] S6. Passivation: Soak the die-cast aluminum in the passivation solution for 2-4 minutes for passivation treatment. The die-cast aluminum forms a protective passivation film to improve the corrosion resistance of the die-cast aluminum.

[0055] The passivation solution includes 10-12% sodium nitrite, 3-10% chromium nitrate, 2-8% organic acid complexing agent, 1-6% polyhydroxy alcohol complexing agent, 1-3% corrosion inhibitor, 1-3% film-forming accelerator, and water;

[0056] S7, water washing: at room temperature, wash the die-cast aluminum with deionized water for 30-40 seconds, and use running water to clean the die-cast aluminum to remove the passivation solution residue;

[0057] S8. Hot water washing: Wash the die-cast aluminum with hot water at a temperature of 60-80℃ for 30-40s to ensure that the die-cast aluminum is thoroughly cleaned to avoid the residual passivation liquid affecting the subsequent use of the die-cast aluminum;

[0058] S9, drying: place the passivated die-cast aluminum in a blast drying oven 1, maintain the drying temperature in the range of 80-90°C, and dry for 5-10 minutes to avoid water marks and spots on the surface of the die-cast aluminum and ensure the surface finish.

[0059] Example 2: This example provides a method for preparing an environmentally friendly aluminum passivation film-forming agent. Figure 1 , including the following steps:

[0060] S1. Degreasing and cleaning: Soak the die-cast aluminum in degreasing liquid for 20-40 minutes. Keep the degreasing liquid at a temperature of 60-80°C to ensure that the oil and impurities are completely removed. Remove the oil, dust and other impurities on the surface of the die-cast aluminum;

[0061] The degreasing liquid includes 8% sodium hydroxide, 1.5% sodium carbonate, 4% sodium phosphate, 2% sodium silicate, and water. The degreasing liquid uses the wettability, permeability, emulsification and dispersibility of the surfactant to remove dirt from the surface of the die-cast aluminum.

[0062] S2. Pickling: Immerse the die-cast aluminum in a pickling solution to remove the oxide scale and oxide layer on the surface of the die-cast aluminum and improve the surface finish to prepare for passivation treatment. The pickling solution includes 15% hydrochloric acid, 1% hexamethylenetetramine, 3% hydrofluoric acid, 10% nitric acid, and water;

[0063] After pickling, the die-cast aluminum is neutralized with a neutralizing solution, which includes 2% ammonia water and water. The die-cast aluminum is fully rinsed with flowing neutralizing solution to remove residual pickling solution and other chemicals to ensure that the surface of the die-cast aluminum is no longer acidic.

[0064] S3. Hot water washing: Wash the die-cast aluminum with hot water at a temperature of 60-80℃ for 30-40s to ensure that the die-cast aluminum is thoroughly cleaned and avoid the residual pickling liquid from affecting the subsequent use of the die-cast aluminum;

[0065] S4. Activation: At room temperature, use 5-10 ml / L of hydrofluoric acid to activate the die-cast aluminum for 20-30 seconds;

[0066] S5. Water washing: Wash the die-cast aluminum with deionized water for 30-40 seconds at room temperature to prevent activation residues from affecting the subsequent use of the die-cast aluminum.

[0067] S6. Passivation: Soak the die-cast aluminum in the passivation solution for 2-4 minutes for passivation treatment. The die-cast aluminum forms a protective passivation film to improve the corrosion resistance of the die-cast aluminum.

[0068] The passivation solution includes 10% sodium nitrite, 3% chromium nitrate, 2% organic acid complexing agent, 1% polyhydroxy alcohol complexing agent, 1% corrosion inhibitor, 1% film-forming accelerator, and water;

[0069] S7, water washing: at room temperature, wash the die-cast aluminum with deionized water for 30-40 seconds, and use running water to clean the die-cast aluminum to remove the passivation solution residue;

[0070] S8. Hot water washing: Wash the die-cast aluminum with hot water at a temperature of 60-80℃ for 30-40s to ensure that the die-cast aluminum is thoroughly cleaned to avoid the residual passivation liquid affecting the subsequent use of the die-cast aluminum;

[0071] S9, drying: place the passivated die-cast aluminum in a blast drying oven 1, maintain the drying temperature in the range of 80-90°C, and dry for 5-10 minutes to avoid water marks and spots on the surface of the die-cast aluminum and ensure the surface finish.

[0072] Example 3: This example provides a method for preparing an environmentally friendly aluminum passivation film-forming agent. Figure 1 , including the following steps:

[0073] S1. Degreasing and cleaning: Soak the die-cast aluminum in degreasing liquid for 20-40 minutes. Keep the degreasing liquid at a temperature of 60-80°C to ensure that the oil and impurities are completely removed. Remove the oil, dust and other impurities on the surface of the die-cast aluminum;

[0074] The degreasing liquid includes 9% sodium hydroxide, 2% sodium carbonate, 4% sodium phosphate, 2% sodium silicate, and water. The degreasing liquid uses the wettability, permeability, emulsification and dispersibility of the surfactant to remove dirt from the surface of the die-cast aluminum.

[0075] S2. Pickling: Immerse the die-cast aluminum in a pickling solution to remove the oxide scale and oxide layer on the surface of the die-cast aluminum and improve the surface finish to prepare for passivation treatment. The pickling solution includes 15% hydrochloric acid, 1% hexamethylenetetramine, 3% hydrofluoric acid, 10% nitric acid, and water;

[0076] After pickling, the die-cast aluminum is neutralized with a neutralizing solution, which includes 2% ammonia water and water. The die-cast aluminum is fully rinsed with flowing neutralizing solution to remove residual pickling solution and other chemicals to ensure that the surface of the die-cast aluminum is no longer acidic.

[0077] S3. Hot water washing: Wash the die-cast aluminum with hot water at a temperature of 60-80℃ for 30-40s to ensure that the die-cast aluminum is thoroughly cleaned and avoid the residual pickling liquid from affecting the subsequent use of the die-cast aluminum;

[0078] S4. Activation: At room temperature, use 5-10 ml / L of hydrofluoric acid to activate the die-cast aluminum for 20-30 seconds;

[0079] S5. Water washing: Wash the die-cast aluminum with deionized water for 30-40 seconds at room temperature to prevent activation residues from affecting the subsequent use of the die-cast aluminum.

[0080] S6. Passivation: Soak the die-cast aluminum in the passivation solution for 2-4 minutes for passivation treatment. The die-cast aluminum forms a protective passivation film to improve the corrosion resistance of the die-cast aluminum.

[0081] The passivation solution includes 11% sodium nitrite, 6.5% chromium nitrate, 5.5% organic acid complexing agent, 3.5% polyhydroxy alcohol complexing agent, 2% corrosion inhibitor, 2% film-forming accelerator, and water;

[0082] S7, water washing: at room temperature, the die-cast aluminum is washed with deionized water for 30-40 seconds, and the die-cast aluminum is cleaned with running water to remove the passivation liquid residue;

[0083] S8. Hot water washing: Wash the die-cast aluminum with hot water at a temperature of 60-80℃ for 30-40s to ensure that the die-cast aluminum is thoroughly cleaned to avoid the residual passivation liquid affecting the subsequent use of the die-cast aluminum;

[0084] S9, drying: place the passivated die-cast aluminum in a blast drying oven 1, maintain the drying temperature in the range of 80-90°C, and dry for 5-10 minutes to avoid water marks and spots on the surface of the die-cast aluminum and ensure the surface finish.

[0085] Example 4: This example provides a method for preparing an environmentally friendly aluminum passivation film-forming agent. Figure 1 , including the following steps:

[0086] S1. Degreasing and cleaning: Soak the die-cast aluminum in degreasing liquid for 20-40 minutes. Keep the degreasing liquid at a temperature of 60-80°C to ensure that the oil and impurities are completely removed. Remove the oil, dust and other impurities on the surface of the die-cast aluminum;

[0087] The degreasing liquid includes 10% sodium hydroxide, 2.5% sodium carbonate, 4% sodium phosphate, 2% sodium silicate, and water. The degreasing liquid uses the wettability, permeability, emulsification and dispersibility of the surfactant to remove dirt from the surface of the die-cast aluminum.

[0088] S2. Pickling: Immerse the die-cast aluminum in a pickling solution to remove the oxide scale and oxide layer on the surface of the die-cast aluminum and improve the surface finish to prepare for passivation treatment. The pickling solution includes 15% hydrochloric acid, 1% hexamethylenetetramine, 3% hydrofluoric acid, 10% nitric acid, and water;

[0089] After pickling, the die-cast aluminum is neutralized with a neutralizing solution, which includes 2% ammonia water and water. The die-cast aluminum is fully rinsed with flowing neutralizing solution to remove residual pickling solution and other chemicals to ensure that the surface of the die-cast aluminum is no longer acidic.

[0090] S3. Hot water washing: Wash the die-cast aluminum with hot water at a temperature of 60-80℃ for 30-40s to ensure that the die-cast aluminum is thoroughly cleaned and avoid the residual pickling liquid from affecting the subsequent use of the die-cast aluminum;

[0091] S4. Activation: At room temperature, use 5-10 ml / L of hydrofluoric acid to activate the die-cast aluminum for 20-30 seconds;

[0092] S5. Water washing: Wash the die-cast aluminum with deionized water for 30-40 seconds at room temperature to prevent activation residues from affecting the subsequent use of the die-cast aluminum.

[0093] S6. Passivation: Soak the die-cast aluminum in the passivation solution for 2-4 minutes for passivation treatment. The die-cast aluminum forms a protective passivation film to improve the corrosion resistance of the die-cast aluminum.

[0094] The passivation solution includes 12% sodium nitrite, 10% chromium nitrate, 8% organic acid complexing agent, 6% polyhydroxy alcohol complexing agent, 3% corrosion inhibitor, 3% film-forming accelerator, and water;

[0095] S7, water washing: at room temperature, the die-cast aluminum is washed with deionized water for 30-40 seconds, and the die-cast aluminum is cleaned with running water to remove the passivation liquid residue;

[0096] S8. Hot water washing: Wash the die-cast aluminum with hot water at a temperature of 60-80℃ for 30-40s to ensure that the die-cast aluminum is thoroughly cleaned to avoid the residual passivation liquid affecting the subsequent use of the die-cast aluminum;

[0097] S9, drying: place the passivated die-cast aluminum in a blast drying oven 1, maintain the drying temperature in the range of 80-90°C, and dry for 5-10 minutes to avoid water marks and spots on the surface of the die-cast aluminum and ensure the surface finish.

[0098] Embodiment 5: Based on Embodiments 1 to 4, see Figure 2-5 This embodiment provides a blast drying oven used in S9, and its structure is as follows:

[0099] A pair of rectangular openings are provided at the bottom of the two side walls of the blast drying box 1, and a movable hinged side door panel 3 is provided inside each rectangular opening. A pair of symmetrically distributed side panels 16 are fixed to the inner bottom wall of the blast drying box 1, and a loading plate 9 is provided on the outer side of each side panel 16. A plurality of equally distributed loading slots are provided on the top surface of each loading plate 9, and a plurality of evenly distributed leakage holes are provided on the inner bottom wall of each loading slot, and die-cast aluminum 23 is placed inside each loading slot.

[0100] In the specific implementation process, Figure 4 and Figure 5 As shown, a pair of first connecting shafts are fixedly provided at the two corners of the top of the side plate 16, and a vertically distributed fixed swing arm 10 is fixedly provided at the outer end of each first connecting shaft, and a pair of penetratingly distributed second connecting shafts are hingedly inserted at the front and rear sides of the loading plate 9, and the inner end of each second connecting shaft is fixedly connected to the bottom end of the corresponding fixed swing arm 10; because the fixed swing arm 10 rotates in parallel, it drives the loading plate 9 and a number of die-cast aluminum 23 to perform intermittent lifting and translation;

[0101] A pair of symmetrically distributed extended ear seats 13 are fixedly provided on the inner bottom wall of the blast drying box 1, and the pair of extended ear seats 13 are located between a pair of side plates 16, and a linkage shaft that is distributed through the top end of each extended ear seat 13 is rotatably inserted, and an active swing arm 12 is fixedly provided at the outer end of each linkage shaft;

[0102] A suspended T-shaped swing arm 14 is provided between the extended ear seat 13 and the side plate 16 on the same side. The top end of the active swing arm 12 is movably hinged to the top end of the T-shaped swing arm 14. A driven swing arm 15 is fixed to the inner end of each first connecting shaft. The two ends of the T-shaped swing arm 14 are movably hinged to the top ends of a pair of driven swing arms 15. Under the joint hinge action of the active swing arm 12 and the T-shaped swing arm 14, the driven swing arm 15, the first connecting shaft, the fixed swing arm 10 and the second connecting shaft are driven to rotate intermittently.

[0103] In the specific implementation process, Figure 4 and Figure 5 As shown, the inner end of each linkage shaft is sleeved with a concentrically fixed driven bevel gear 11, a transversely distributed connecting plate 18 is fixed between the middle and upper parts of a pair of extended ear seats 13, and an intermittent shaft distributed through the middle of the connecting plate 18 is rotatably inserted, and the top end of the intermittent shaft is sleeved with a concentrically fixed driving bevel gear 17, and the driving bevel gear 17 is respectively meshed and connected with a pair of driven bevel gears 11, and the intermittent plate 19 drives the intermittent shaft and the driving bevel gear 17 to intermittently rotate, and the driving bevel gear 17 is then meshed to drive the driven bevel gear 11, the linkage shaft, and the active swing arm 12 to intermittently rotate;

[0104] A transversely distributed T-shaped plate 21 is fixedly disposed between the middle and lower parts of a pair of extended ear seats 13, a circular through hole is provided at the front end of the T-shaped plate 21, a servo motor 22 with an output end facing upward is fixedly disposed inside the circular through hole, a limit cam 20 is fixedly disposed at the motor shaft end of the servo motor 22, a triangular notch is provided at the front end of the limit cam 20, a vertically distributed limit pin is fixedly disposed at the front end of the triangular notch, and the motor shaft of the servo motor 22 drives the limit cam 20 and the limit pin to rotate synchronously;

[0105] The bottom end of the intermittent shaft is sleeved with a concentrically fixed intermittent disk 19, and a number of evenly distributed arc-shaped notches are provided on the outer surface of the intermittent disk 19, and a U-shaped notch is provided between an adjacent pair of arc-shaped notches. The top surface of the triangular notch slides against the bottom surface of the intermittent disk 19, and the outer ring surface of the limit cam 20 slides against the arc-shaped notch, and the top end of the limit pin slides against the corresponding U-shaped notch and drives the intermittent disk 19 to rotate. The limit cam 20 and the limit pin alternately form a limiting effect with the arc-shaped notch and the U-shaped notch on the intermittent disk 19, and drive the intermittent disk 19 to rotate intermittently.

[0106] It should be noted that: in this embodiment, the four corners of the top surface of the blast drying box 1 are fixedly provided with a through-distributed fixed ring 5, and the interior of each fixed ring 5 is fixedly provided with a drying fan 4 with an output wind direction, and a pair of fan control modules 6 are fixedly provided on both sides of the top surface of the blast drying box 1, and the fan control modules 6 are electrically connected to the adjacent pair of drying fans 4, and the bottom corners of the front and rear sides of the blast drying box 1 are fixedly provided with a through-distributed return pipe 2, and the top end of each return pipe 2 is bent downward and faces the top end of the corresponding fixed ring 5; under the action of the pair of fan control modules 6, the two pairs of drying fans 4 are controlled to blow downward, and the outside air passes through the continuous S-shaped heating wire 8 to be heated and then blown onto the plurality of die-cast aluminums 23, and then the hot air flows along the return pipe 2 and flows back into the fixed ring 5 to form a circulation flow, and the plurality of die-cast aluminums 23 are continuously dried;

[0107] A pair of symmetrically distributed heating control modules 7 are fixed on the top of the two side walls of the blast drying box 1, and a pair of symmetrically distributed continuous S-shaped heating wires 8 are fixed on the top of the two side walls inside the blast drying box 1. Both ends of the continuous S-shaped heating wires 8 penetrate the side walls of the blast drying box 1 and extend to the outside. Both ends of the heating control module 7 are electrically connected to both ends of the adjacent continuous S-shaped heating wires 8; under the action of the pair of heating control modules 7, the continuous S-shaped heating wires 8 are controlled to heat, and under the heating action of the continuous S-shaped heating wires 8, the surrounding air is heated to a suitable temperature.

[0108] Specifically, the working principle and operation method of the blast drying oven are as follows:

[0109] Step 1: open a pair of side door panels 3, place a plurality of die-cast aluminums 23 in a plurality of loading slots respectively, and under the driving action of the servo motor 22, the motor shaft of the servo motor 22 drives the limit cam 20 and the limit pin shaft to rotate synchronously, and the limit cam 20 and the limit pin shaft alternately form a limit effect with the arc-shaped notch and the U-shaped notch on the intermittent disk 19, and the intermittent disk 19 is moved to rotate intermittently;

[0110] Step 2: The intermittent disc 19 drives the intermittent shaft and the active bevel gear 17 to rotate intermittently. The active bevel gear 17 then meshes to drive the driven bevel gear 11, the linkage shaft, and the active swing arm 12 to rotate intermittently. Under the joint articulation of the active swing arm 12 and the T-shaped swing arm 14, the driven swing arm 15, the first connecting shaft, the fixed swing arm 10, and the second connecting shaft are driven to rotate intermittently. Since the fixed swing arm 10 rotates in parallel, the loading plate 9 and the plurality of die-cast aluminums 23 are driven to perform intermittent lifting and translation, so that they are briefly paused at the highest point, the lowest point, the front end, and the rear end.

[0111] Step three, under the action of a pair of heating control modules 7, the continuous S-shaped heating wire 8 is controlled to heat up. Under the heating action of the continuous S-shaped heating wire 8, the surrounding air is heated to a suitable temperature. Under the action of a pair of fan control modules 6, two pairs of drying fans 4 are controlled to blow air downward. Under the action of the drying fans 4, the outside air passes through the continuous S-shaped heating wire 8 and is heated before being blown onto a number of die-cast aluminums 23. Then the hot air flows along the reflux pipe 2 and refluxes into the fixed ring 5 to form a circulating flow, thereby continuously drying a number of die-cast aluminums 23.

[0112] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing an environmentally friendly aluminum passivation film-forming agent, comprising the following steps: S1. Degreasing and cleaning: Soak the die-cast aluminum in degreasing liquid for 20-40 minutes. Keep the degreasing liquid at a temperature of 60-80°C to ensure that the oil and impurities are completely removed. Remove the oil, dust and other impurities on the surface of the die-cast aluminum; The degreasing liquid includes 8-10% sodium hydroxide, 1.5-2.5% sodium carbonate, 4% sodium phosphate, 2% sodium silicate, and water. The degreasing liquid uses the wettability, permeability, emulsification and dispersibility of the surfactant to remove dirt from the surface of the die-cast aluminum. S2. Pickling: Immerse the die-cast aluminum in a pickling solution to remove the oxide scale and oxide layer on the surface of the die-cast aluminum and improve the surface finish to prepare for passivation treatment. The pickling solution includes 15% hydrochloric acid, 1% hexamethylenetetramine, 3% hydrofluoric acid, 10% nitric acid, and water; After pickling, the die-cast aluminum is neutralized with a neutralizing solution, which includes 2% ammonia water and water. The die-cast aluminum is fully rinsed with flowing neutralizing solution to remove residual pickling solution and other chemicals to ensure that the surface of the die-cast aluminum is no longer acidic. S3. Hot water washing: Wash the die-cast aluminum with hot water at a temperature of 60-80℃ for 30-40s to ensure that the die-cast aluminum is thoroughly cleaned and avoid the residual pickling liquid from affecting the subsequent use of the die-cast aluminum; S4. Activation: At room temperature, use 5-10 ml / L of hydrofluoric acid to activate the die-cast aluminum for 20-30 seconds; S5. Water washing: Wash the die-cast aluminum with deionized water for 30-40 seconds at room temperature to prevent activation residues from affecting the subsequent use of the die-cast aluminum. S6. Passivation: Soak the die-cast aluminum in the passivation solution for 2-4 minutes for passivation treatment. The die-cast aluminum forms a protective passivation film to improve the corrosion resistance of the die-cast aluminum. The passivation solution includes 10-12% sodium nitrite, 3-10% chromium nitrate, 2-8% organic acid complexing agent, 1-6% polyhydroxy alcohol complexing agent, 1-3% corrosion inhibitor, 1-3% film-forming accelerator, and water; S7, water washing: at room temperature, wash the die-cast aluminum with deionized water for 30-40 seconds, and use running water to clean the die-cast aluminum to remove the passivation solution residue; S8. Hot water washing: Wash the die-cast aluminum with hot water at a temperature of 60-80℃ for 30-40s to ensure that the die-cast aluminum is thoroughly cleaned to avoid the residual passivation liquid affecting the subsequent use of the die-cast aluminum; S9, drying: placing the passivated die-cast aluminum in a blast drying oven (1), maintaining the drying temperature in the range of 80-90° C., and drying for 5-10 minutes to avoid water marks and spots on the surface of the die-cast aluminum and ensure surface smoothness; In step S9, a pair of rectangular openings are provided at the bottom of the two side walls of the blast drying box (1), each of the rectangular openings is provided with a movable hinged side door panel (3), a pair of symmetrically distributed side panels (16) are fixedly provided on the inner bottom wall of the blast drying box (1), a loading plate (9) is provided on the outer side of each of the side panels (16), a plurality of equally distributed loading slots are provided on the top surface of each of the loading plates (9), a plurality of evenly distributed leakage holes are provided on the inner bottom wall of each of the loading slots, and die-cast aluminum (23) is placed inside each of the loading slots.

2. The method for preparing an environmentally friendly aluminum passivation film-forming agent according to claim 1, characterized in that: The degreasing liquid comprises 9% of sodium hydroxide, 2% of sodium carbonate, 4% of sodium phosphate, 2% of sodium silicate and water.

3. The method for preparing an environmentally friendly aluminum passivation film-forming agent according to claim 1, characterized in that: The passivation solution comprises 11% sodium nitrite, 6.5% chromium nitrate, 5.5% organic acid complexing agent, 3.5% polyhydroxy alcohol complexing agent, 2% corrosion resist, 2% film-forming accelerator and water.

4. The method for preparing an environmentally friendly aluminum passivation film-forming agent according to claim 1, characterized in that: A pair of first connecting shafts are fixedly provided at the two corners of the top of the side plate (16), and a vertically distributed fixed swing arm (10) is fixedly provided at the outer end of each of the first connecting shafts. A pair of penetrating second connecting shafts are hingedly inserted at the front and rear sides of the loading plate (9), and the inner end of each of the second connecting shafts is fixedly connected to the bottom end of the corresponding fixed swing arm (10).

5. The method for preparing an environmentally friendly aluminum passivation film-forming agent according to claim 4, characterized in that: A pair of symmetrically distributed extended ear seats (13) are fixedly provided on the inner bottom wall of the blast drying box (1), and the pair of extended ear seats (13) are located between a pair of side plates (16). A linkage shaft that runs through the top end of each of the extended ear seats (13) is rotatably inserted, and an active swing arm (12) is fixedly provided on the outer end of each of the linkage shafts.

6. The method for preparing an environmentally friendly aluminum passivation film-forming agent according to claim 5, characterized in that: A suspended T-shaped swing arm (14) is provided between the extended ear seat (13) and the side plate (16) on the same side, the top end of the active swing arm (12) is movably hinged to the top end of the T-shaped swing arm (14), a driven swing arm (15) is fixedly provided at the inner end of each of the first connecting shafts, and both ends of the T-shaped swing arm (14) are movably hinged to the top ends of a pair of driven swing arms (15).

7. The method for preparing an environmentally friendly aluminum passivation film-forming agent according to claim 6, characterized in that: The inner end of each linkage shaft is sleeved with a concentrically fixed driven bevel gear (11); a transversely distributed connecting plate (18) is fixed between the middle and upper parts of a pair of extended ear seats (13); an intermittent shaft that is rotatably inserted through the middle of the connecting plate (18); a concentrically fixed driving bevel gear (17) is sleeved on the top end of the intermittent shaft; the driving bevel gear (17) is respectively meshed and connected with a pair of driven bevel gears (11).