Novel monocrystalline silicon texturing solution and preparation method thereof

Through the use of the new single crystal silicon velvet making solution, the problems of long velvet making time, high safety risks and high reflectivity are solved, and a more efficient and environmentally friendly velvet making process is achieved, forming a uniform small-sized pyramid structure, and improving solar energy The photoelectric conversion efficiency and battery life of the battery.

CN118910725APending Publication Date: 2024-11-08HEBEI NORMAL UNIV FOR NATTIES
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411103670.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing monocrystalline silicon solar cell velvet making process has problems such as long velvet making time, high safety risks, high reflectivity, and short battery life. The traditional alkali alcohol system is easy to evaporate, has a large environmental pollution, and it is difficult to accurately regulate the surface of the silicon wafer. Pyramid structure.

Method used

A new single crystal silicon velvet-making solution is adopted, which contains nucleating agent, defoaming agent, main corrosion inhibitor, secondary corrosion inhibitor, complexing agent, suede modification agent and surfactant. The preparation method is prepared by stirring evenly. Inorganic lye is avoided, organic lye and deionized water are used, the velvet-making temperature is 65℃ and the velvet-making time is 180s, forming a uniform small-sized pyramid structure, reducing reflectivity and improving photoelectric conversion efficiency.

Benefits of technology

Significantly shortens the time of velvet making, reduces reflectivity, improves battery life, reduces production safety risks, improves photoelectric conversion efficiency, reduces chemicals, reduces environmental pollution, and the additives are non-toxic and have good environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910725A_ABST
    Figure CN118910725A_ABST
Patent Text Reader

Abstract

The invention relates to a novel monocrystalline silicon texturing solution and a preparation method thereof. The novel monocrystalline silicon texturing solution comprises a nucleating agent, a defoaming agent, a main corrosion inhibitor, an auxiliary corrosion inhibitor, a complexing agent, a texturing modifier, a surfactant, organic alkali liquor and the balance of deionized water. The invention has the following advantages: firstly, the service life is long, and the volatilization amount is low, so that the supplement amount is small, and the usage amount of chemical substances is obviously reduced; and secondly, the texturing liquid and the waste liquid thereof are light in color, extremely low in chemical oxygen demand and very small in influence on the environment, and meet the requirement of green production. In addition, according to the texturing technology, the production process is simplified, the texturing time is shortened, and meanwhile the excellent texturing effect is ensured. Specifically, through the texturing process provided by the invention, a pyramid-shaped textured structure which is smaller in size and more uniform in distribution can be obtained, and the surface reflectivity of a silicon wafer is effectively reduced, so that the photoelectric conversion efficiency of a solar cell is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of single crystal silicon solar cells, in particular to a novel single crystal silicon texturing solution and a preparation method thereof. Background Art

[0002] As people pay more attention to energy issues in recent years, solar cells, as semiconductor devices that can convert solar energy into light energy, have developed rapidly. In the production of solar cells, the performance and photoelectric conversion rate of silicon wafer solar cells are closely related to the surface structure of solar cells. Chemical etching is the lowest cost and most widely used method for preparing the textured surface structure of single crystal silicon. Therefore, in the manufacturing process, chemical etching of silicon wafers is an important process, which aims to reduce the surface reflectivity of silicon wafers, increase light absorption, and increase the density of photogenerated carriers, thereby improving the photoelectric conversion rate of solar cells. The basic principle of single crystal silicon texture can be simply attributed to the anisotropic corrosion caused by the difference in the dangling bond and back bond structure on the surface of the silicon wafer. Since the corrosion rate of silicon on the (110) and (100) crystal planes is much greater than the corrosion rate of the (111) crystal plane, after a certain period of corrosion, four pyramid structures composed of (111) planes are left on the surface of the (100) single crystal silicon wafer. Its chemical reaction formula can be summarized as:

[0003] Si+2NaOH+H2O→Na2SiO3+H2↑;

[0004] The general process of the reaction is: (1) the reactants diffuse to the silicon surface; (2) the silicon surface adsorbs reactive and non-reactive substances / ions; (3) the surface reacts (silicon oxidation); (4) the reaction products desorb; and (5) the reaction products diffuse from the silicon surface into the solution.

[0005] The traditional texturing method mainly relies on the alkali (KOH or NaOH) alcohol (isopropanol) system, but this process has great defects. First, the texturing time is long, and the reaction generally takes 30 to 40 minutes, which increases the safety risk; secondly, the boiling point of isopropanol is relatively low at 82.4°C, close to the reaction temperature of 80°C, and it is easy to volatilize, so it is necessary to continuously add isopropanol during the reaction process to maintain its concentration, which is not good for the environment; thirdly, isopropanol has a small molecular weight and weak adsorption capacity for silicon, and cannot play a full masking role, thus affecting the texturing rate, resulting in a larger velvet surface size, a higher reflectivity of the texturing silicon wafer, and it is difficult to guarantee the texturing effect; finally, due to the problem of inorganic alkali ionization, there are metal ions in the reaction solution, and these metal ions will form a composite center to affect the minority carrier lifetime of the single crystal silicon wafer.

[0006] In order to improve the alkali-alcohol process, researchers have gradually proposed sodium carbonate, sodium bicarbonate, sodium phosphate, ethylenediamine and tetramethylammonium hydroxide as etchants to replace sodium hydroxide or potassium hydroxide to reduce reflectivity, but the velvet uniformity and reaction reproducibility produced by these substitutes are poor, the reaction time is long and the system stability is poor. In order to further optimize the velvet process, some researchers have proposed a strategy of organic acid compound surfactant assisted nucleation. This strategy greatly improves the velvet uniformity and reduces the reflectivity, but still requires a small amount of alcohol compounds to assist nucleation, and the reaction time is still long, and the stability is not ideal. CN112144122A discloses a velvet additive suitable for large-size single crystal silicon wafers, which contains: 0.5-10% of the main nucleating agent, 0.2-5% of the supplementary nucleating agent, 0.01-0.1% of the branched dispersant, 0.05-0.5% of the defoaming agent, and the balance is water. It uses hydrolyzed sodium polyacrylonitrile as the main nucleating agent and polyamino acid as the supplementary nucleating agent, which solves the problem of unevenness within the large-sized silicon wafer after texturing; the texturing reflectivity is low and the texturing time is short. CN111321471A discloses a low-weight-loss single-crystal silicon texturing additive, which includes: 0.01-1% polysaccharide sulfonate, 0.1-3% degassing dispersant, 0.01-1% corrosion inhibitor, 0.05-0.5% water-soluble polymer protective agent, 0.05-2% alkali, and the balance is water. It overcomes the defects of low production capacity, heavy weight loss of texturing silicon wafers, high alkali consumption, and short service life in the prior art. The texturing agents disclosed in the above technology still have technical problems such as high safety risks, long texturing time, extremely volatile alcohols, low texturing rate, poor uniformity of the surface of the texturing silicon wafer, and short battery life to varying degrees. Therefore, it is imperative to develop green and environmentally friendly texturing additives with high boiling points and low volatility, and efficient, stable and fast texturing.

[0007] CN116144362A discloses an alcohol-free monocrystalline silicon texturing additive, which includes, by weight: 0.1-20 parts of corrosion inhibitor; 0.1-10 parts of surfactant; 0.5-30 parts of small molecule sugar alcohol; 30-70 parts of inorganic alkali solution; 30-50 parts of deionized water. It uses an environmentally friendly high-boiling point surfactant, which solves the problem of toxicity and volatility of traditional low-boiling point alcohols such as isopropyl alcohol, is green and environmentally friendly, saves time and effort, and saves costs. CN111647951A discloses an environmentally friendly single crystal silicon texturing additive, which comprises, by weight percentage: 0.01-0.5% sodium lignin sulfonate, 0.02-1.2% polyacrylic acid, 0.0001-0.01% methylene bis naphthalene sulfonic acid, 0.001-0.01% polyethylene glycol, 0.01-2% L-cysteine, and 96-99% water. The texturing additive is added to a 1%-2% sodium hydroxide or potassium hydroxide solution, and mixed evenly at a temperature of 20-80°C. The texturing liquid of the invention has a small amount of volatility, a small amount of addition, and a very low amount of chemical substances. The texturing liquid and its waste liquid are light in color, and the chemical oxygen demand is very low. The environmental pollution is small, the production cost is reduced, and the texturing effect is good. Although the texturing agent disclosed in the above technology solves the technical problems of high safety risk of previous texturing liquid, long texturing time, extremely volatile alcohols, low texturing rate, poor uniformity of texturing silicon wafer surface, and short battery life, it still uses traditional organic alkali as the core corrosion liquid. Inorganic alkali ionization produces metal ions. These metal ions will form a composite center that affects the minority carrier life of the single crystal silicon wafer. In addition, the regulation of the inverted pyramid structure on the surface of single crystal silicon needs to be improved. Therefore, it is imperative to develop a texturing liquid that can improve battery life and accurately regulate the inverted pyramid structure on the surface of single crystal silicon. Summary of the invention

[0008] In order to improve the photoelectric conversion efficiency of monocrystalline silicon cells, the present invention proposes a new type of monocrystalline silicon texturing solution and its preparation method by finding a replacement for the traditional alkali (KOH or NaOH) alcohol (isopropanol) system and adding new substances to improve the photoelectric conversion efficiency of monocrystalline silicon cells in view of the shortcomings of the prior art. The inverted pyramid structure formed after texturing is moderate in size and more uniform, thereby effectively reducing the reflectivity after texturing, improving the photoelectric conversion efficiency of the cell, and extending the battery life. In addition, the production safety risk is reduced and the texturing time is shortened.

[0009] In order to achieve the above technical objectives, the technical solution adopted by the present invention is:

[0010] A novel monocrystalline silicon texturing solution comprises the following components in percentage by mass:

[0011] 0.8% to 1.3% nucleating agent, 0.2% to 0.3% defoaming agent, 0.5% primary corrosion inhibitor, 0.03% to 0.15% secondary corrosion inhibitor, 0.05% to 0.08% complexing agent, 0.1% to 0.2% suede modifier, 0.25% surfactant, 3% to 5% organic alkali solution, and the balance is deionized water. The mixed solution is mixed evenly by a stirring device and used as the suede liquid for photovoltaic monocrystalline silicon panels.

[0012] Furthermore, the novel single crystal silicon texturing solution does not contain inorganic alkali solution, and the inorganic alkali solution refers to potassium hydroxide, sodium hydroxide, etc. but is not limited thereto.

[0013] Furthermore, the nucleating agent is a small molecule sugar or a sugar alcohol.

[0014] Furthermore, the nucleating agent is preferably one or more of erythrose, arabinose, glucose, fructose, galactose, sucrose, trehalose, melibiose, fucose, rhamnose, cellobiose, gentiobiose, cellotriose, gentiotriose, melezitose, raffinose, stevioside, stachyose, lactitol, maltitol, isomalt, erythritol, xylitol, mannitol and sorbitol.

[0015] Furthermore, the mass percentage of the nucleating agent is preferably 0.9% to 1.2%.

[0016] Furthermore, the defoaming agent is one or more of polyvinyl alcohol, polydimethylsiloxane, lauric acid, and palmitic acid.

[0017] Furthermore, the defoaming agent preferably has a molecular weight of 5000-50000.

[0018] Furthermore, the mass percentage of the defoaming agent is preferably 0.25% to 0.3%.

[0019] Furthermore, the main corrosion inhibitor is a catechol derivative compound, selected from one or more of catechol, o-methoxyphenol and 2-methoxy-4-methylphenol, catecholamine, and bis-catechol ligands.

[0020] Furthermore, the mass percentage of the main corrosion inhibitor is preferably 0.5%.

[0021] Furthermore, the secondary corrosion inhibitor is an amine, an alcohol amine, an organic weak acid, or an acid sodium salt; selected from one or more of dopamine hydrochloride, amine wanda, L-cysteine, ascorbic acid, acetic acid, propionic acid, benzoic acid, oxalic acid, salicylic acid, sodium silicate, sodium formate, sodium acetate, sodium lactate, sodium oxalate, sodium succinate, sodium benzoate, sodium phenylacetate, sodium isophthalate, sodium lignin sulfonate, and sodium methylene bisnaphthalene sulfonate.

[0022] Furthermore, the secondary corrosion inhibitor is more preferably one or more of dopamine hydrochloride, amine wanda, L-cysteine, ascorbic acid, sodium silicate, sodium acetate, sodium lactate, sodium lignin sulfonate, and sodium methylene bisnaphthalene sulfonate.

[0023] Furthermore, the mass percentage of the secondary corrosion inhibitor is preferably 0.05% to 0.15%.

[0024] Furthermore, the complexing agent is one or more of tetrasodium ethylenediaminetetraacetate, triethanolamine, sodium nitrilotriacetate, and sodium diethylenetriaminepentacarboxylate.

[0025] Furthermore, the mass percentage of the complexing agent is preferably 0.06% to 0.07%.

[0026] Furthermore, the suede modifying agent is one or more of polyethylene glycol, polypropylene glycol, β-cyclodextrin, xylan, modified starch, and betaine.

[0027] Furthermore, the polyethylene glycol preferably has a molecular weight of 200 or 400.

[0028] Furthermore, the polypropylene glycol preferably has a molecular weight of 400, 1000, 2000, or 4000.

[0029] Furthermore, the mass percentage of the suede finishing agent is preferably 0.17-0.2%.

[0030] Furthermore, the surfactant is an alcohol nonionic surfactant.

[0031] Furthermore, the surfactant is an alcohol nonionic surfactant, selected from one or more of fatty alcohol polyoxyethylene ether AEO-7, fatty alcohol polyoxyethylene ether AEO-9, alkylphenol polyoxyethylene ether OP-10, Tween 20 and Tween 80.

[0032] Furthermore, the mass percentage of the surfactant is preferably 0.25%.

[0033] Furthermore, the organic alkali solution is tetramethylguanidine.

[0034] Furthermore, the mass percentage of the organic alkali solution is preferably 4.5% to 5%.

[0035] In order to achieve the above technical purpose, another technical solution adopted by the present invention is:

[0036] A novel method for preparing a monocrystalline silicon texturing solution includes a texturing solution preparation method and a monocrystalline silicon wafer surface texturing method, specifically:

[0037] A. Preparation of texturing liquid: Add nucleating agent, defoaming agent, primary corrosion inhibitor, secondary corrosion inhibitor, complexing agent, suede modifier, surfactant and organic alkali solution into deionized water according to mass ratio, and stir evenly to obtain texturing liquid;

[0038] B. Use a paddle stirrer, propeller stirrer, turbine stirrer, anchor stirrer, frame stirrer, ribbon stirrer, magnetic stirrer, electric heater, forced mixer, concrete mixer, vertical mixer, new mixer or homogenizing equipment (such as multi-energy high-speed homogenizing emulsifier, high-shear mixing emulsifier) ​​to fully mix the texturing liquid;

[0039] C. Texturing: Immerse the single crystal silicon wafer in the texturing liquid for surface texturing. The texturing temperature is 65°C and the texturing time is 180s.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] 1. Nucleating agents (small molecule sugars or sugar alcohols) contain a large number of hydroxyl groups, which can be adsorbed on the silicon surface through hydrogen bonding or chelation. They can serve as the starting point for nucleation, effectively regulating the distribution of the velvet "pyramids" and forming a good light-trapping structure on the surface of the silicon wafer. At the same time, they can also effectively reduce the surface tension of the solution, accelerate dehydrogenation, avoid the generation of white spots, and promote the formation of uniform and dense pyramids. They can also reduce the contact between hydroxyl groups and the silicon surface, achieving the effect of slowing down the etching rate and controlling weight loss.

[0042] 2. The defoaming agent (polyvinyl alcohol) effectively adjusts the viscosity and hydrophilicity of the additive, promotes the rapid detachment of hydrogen bubbles generated during the alkali corrosion of silicon, and avoids the formation of bubble marks, white spots and patterns on the velvet surface of the produced single crystal silicon.

[0043] 3. The presence of hydroxyl groups in the main corrosion inhibitor (catechol) can be adsorbed on the surface of single crystal silicon, reducing the number of OH- adsorbed on the surface of single crystal silicon, playing a role in reducing the reaction rate, thereby obtaining a uniform and dense velvet surface.

[0044] 4. Among the secondary corrosion inhibitors, sodium silicate, sodium formate, sodium acetate, and sodium lactate can reduce the reaction speed in the initial stage of the reaction, form a better velvet surface, reduce the corrosion of single-crystal silicon wafers, and shorten the velvet making time; the nitrogen atoms contained in amine and amino acid molecules can form hydrogen bonds with the phenolic hydroxyl groups in catechol derivative compounds. The two synergistically greatly inhibit the oxidation of catechol derivative corrosion inhibitors, improve molecular stability, and effectively improve the stability of velvet additives and velvet making systems. Secondary corrosion inhibitors can also be used as velvet modifiers to further improve the density of the velvet surface and reduce reflectivity.

[0045] 5. Complexing agents are used to capture metal ions and increase the cleanliness of the silicon wafer surface.

[0046] 6. The velvet modifier can improve the density and uniformity of the pyramids, forming a large number of small-sized positive pyramids. This can make the surface velvet of the single-crystal silicon wafer very uniform and the reflectivity very low, which is beneficial to the passivation effect of silicon nitride coating and improves the open circuit voltage and photoelectric conversion efficiency of the battery; the velvet making time is greatly shortened, and the output of single-crystal silicon wafers per unit velvet making time is increased; the reduction in corrosion can greatly improve the utilization rate of chemicals, reduce emissions, reduce production costs, and reduce the fragmentation rate of single-crystal silicon wafers after velvet making.

[0047] 7. Surfactants play a role in finely controlling the corrosion process of microstructure formation.

[0048] 8. After using the additive of the present invention, compared with the case where no additive is added or isophthalic acid is used as an additive, the texturing time can be shortened and the texturing effect is significantly improved. The velvet pyramids are of moderate size and more evenly distributed, which significantly reduces the reflectivity of the silicon wafer. It also has a very significant effect on the final battery cell, improving the photoelectric conversion efficiency and service life of the battery cell. In addition, the additive of the present invention is non-toxic, non-corrosive, non-irritating, has no combustion and explosion hazards, and is harmless to the human body and the environment. The texturing liquid has a long life, low volatility, low replenishment, and extremely low chemical usage. The texturing liquid and its waste liquid are light in color, which has little pollution to the environment and reduces production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 This is a scanning electron microscope image of the product after the surface of the single crystal silicon wafer in Example 8 was textured. DETAILED DESCRIPTION

[0050] Now, in conjunction with specific embodiments, the technical solutions in the present invention are explained in detail. It should be noted that the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0051] Embodiment 1:

[0052] A. Prepare the texturing liquid: take 8g of maltitol, 2.5g of polyvinyl alcohol, 5g of catechol, 0.3g of amine wanda, 0.2g of L-cysteine, 0.4g of sodium silicate, 0.6g of sodium lignin sulfonate, 0.8g of tetrasodium ethylenediaminetetraacetic acid, 1g of polyethylene glycol, 1g of β-cyclodextrin, 2.5g of Tween-20, 45g of tetramethylguanidine, and 932.7g of deionized water.

[0053] B. Use a paddle stirrer to mix thoroughly.

[0054] C. Texturing: Immerse the single crystal silicon wafer in the texturing liquid for surface texturing. The texturing temperature is 65°C and the texturing time is 180s.

[0055] Embodiment 2:

[0056] A. Prepare the texturing solution: take 13g erythrose, 2.5g polyvinyl alcohol, 5g o-methoxyphenol, 0.4g dopamine hydrochloride, 0.35g ascorbic acid, 0.15g sodium acetate, 0.5g triethanolamine, 1g polypropylene glycol, 0.5g β-cyclodextrin, 2.5g Tween-80, 40g tetramethylguanidine, and 934.1g deionized water.

[0057] B. Use a frame mixer to mix it thoroughly.

[0058] C. Texturing: Immerse the single crystal silicon wafer in the texturing liquid for surface texturing. The texturing temperature is 65°C and the texturing time is 180s.

[0059] Embodiment 3:

[0060] A. Prepare the texturing solution: take 10.5g of mannitol, 3g of polydimethylsiloxane, 5g of 2-methoxy-4-methylphenol, 0.1g of amine wanda, 0.1g of benzoic acid, 0.1g of sodium lactate, 0.65g of sodium nitrilotriacetate, 0.3g of polyethylene glycol, 0.7g of modified starch, 2.5g of fatty alcohol polyoxyethylene ether AEO-7, 50g of tetramethylguanidine, and 927g of deionized water.

[0061] B. Use a magnetic stirrer to mix it thoroughly.

[0062] C. Texturing: Immerse the single crystal silicon wafer in the texturing liquid for surface texturing. The texturing temperature is 65°C and the texturing time is 180s.

[0063] Example 4

[0064] A. Prepare the texturing liquid: take 8g arabinose, 2g lauric acid, 5g catecholamine, 0.3g amine wanda, 0.2g oxalic acid, 0.4g sodium isophthalate, 0.8g sodium diethylenetriamine pentacarboxylate, 0.5g polypropylene glycol, 0.5g betaine, 2.5g fatty alcohol polyoxyethylene ether AEO-9, 30g tetramethylguanidine, and 949.8g deionized water.

[0065] B. Use a paddle stirrer to mix thoroughly.

[0066] C. Texturing: Immerse the single crystal silicon wafer in the texturing liquid for surface texturing. The texturing temperature is 65°C and the texturing time is 180s.

[0067] Example 5

[0068] A. Prepare the texturing liquid: take 8kg of maltitol, 2.5kg of polyvinyl alcohol, 5kg of catechol, 0.3kg of amine wanda, 0.2kg of L-cysteine, 0.4kg of sodium silicate, 0.6kg of sodium lignin sulfonate, 0.8kg of tetrasodium ethylenediaminetetraacetic acid, 1kg of polyethylene glycol, 1kg of β-cyclodextrin, 2.5kg of Tween-20, 45kg of tetramethylguanidine, and 932.7kg of deionized water.

[0069] B. Use a paddle stirrer to mix thoroughly.

[0070] C. Texturing: Immerse the single crystal silicon wafer in the texturing liquid for surface texturing. The texturing temperature is 65°C and the texturing time is 180s.

[0071] Example 6

[0072] A. Prepare the texturing solution: take 4.5g trehalose and 6g sucrose, 2g polydimethylsiloxane, 5g o-methoxyphenol, 0.15g ascorbic acid and 0.15g sodium benzoate, 0.2g salicylic acid, 0.4g sodium succinate, 0.65g triethanolamine, 1g polyethylene glycol, 1g xylan, 2.5g alkylphenol polyoxyethylene ether OP-10, 40g tetramethylguanidine, and 936.5g deionized water.

[0073] B. Use a paddle stirrer to mix thoroughly.

[0074] C. Texturing: Immerse the single crystal silicon wafer in the texturing liquid for surface texturing. The texturing temperature is 65°C and the texturing time is 180s.

[0075] Example 7

[0076] A. Prepare the texturing liquid: take 8kg of maltitol, 2.5kg of polyvinyl alcohol, 5kg of catechol, 0.3kg of amine wanda, 0.2kg of L-cysteine, 0.4kg of sodium silicate, 0.6kg of sodium lignin sulfonate, 0.8kg of tetrasodium ethylenediaminetetraacetic acid, 1kg of polyethylene glycol, 1kg of β-cyclodextrin, 2.5kg of Tween-20, 45kg of tetramethylguanidine, and 932.7kg of deionized water.

[0077] B. Use a vertical mixer to mix it thoroughly.

[0078] C. Texturing: Immerse the single crystal silicon wafer in the texturing liquid for surface texturing. The texturing temperature is 65°C and the texturing time is 180s.

[0079] Example 8

[0080] A. Prepare the texturing solution: take 13g erythrose, 2.5g polyvinyl alcohol, 5g o-methoxyphenol, 0.4g dopamine hydrochloride, 0.35g ascorbic acid, 0.15g sodium acetate, 0.5g triethanolamine, 1g polypropylene glycol, 1g β-cyclodextrin, 2.5g Tween-80, 40g tetramethylguanidine, and 933.6g deionized water.

[0081] B. Use a high-speed homogenizer to mix them thoroughly.

[0082] C. Texturing: Immerse the single crystal silicon wafer in the texturing liquid for surface texturing. The texturing temperature is 65°C and the texturing time is 180s.

[0083] Example 9

[0084] A. Prepare the texturing liquid: take 13g erythrose, 1.5g polyvinyl alcohol and 1.5g lauric acid, 5g o-methoxyphenol, 0.4g dopamine hydrochloride, 0.35g ascorbic acid, 0.15g sodium acetate, 0.5g triethanolamine, 1g polypropylene glycol, 0.5g β-cyclodextrin, 2.5g Tween-80, 40g tetramethylguanidine, and 933.6g deionized water.

[0085] B. Use a frame mixer to mix it thoroughly.

[0086] C. Texturing: Immerse the single crystal silicon wafer in the texturing liquid for surface texturing. The texturing temperature is 65°C and the texturing time is 180s.

[0087] Example 10

[0088] A. Prepare the texturing solution: take 10.5g trehalose, 2.5g polyvinyl alcohol, 5g catechol, 0.3g amine wanda, 0.2g salicylic acid, 0.4g sodium succinate, 0.65g tetrasodium ethylenediaminetetraacetic acid, 1g polyethylene glycol, 0.5g xylan, 2.5g alkylphenol polyoxyethylene ether OP-10, 40g tetramethylguanidine, and 936.5g deionized water.

[0089] B. Use a paddle stirrer to mix thoroughly.

[0090] C. Texturing: Immerse the single crystal silicon wafer in the texturing liquid for surface texturing. The texturing temperature is 65°C and the texturing time is 180s.

[0091] Embodiment 11

[0092] A. Prepare the texturing solution: 8g galactose, 2g polyvinyl alcohol, 5g o-methoxyphenol, 0.1g dopamine hydrochloride, 0.05g ascorbic acid, 0.15g sodium acetate, 0.5g triethanolamine, 0.6g polypropylene glycol, 0.4g β-cyclodextrin, 2.5g Tween-80, 30g tetramethylguanidine, and 950.7g deionized water.

[0093] B. Use a frame mixer to mix it thoroughly.

[0094] C. Texturing: Immerse the single crystal silicon wafer in the texturing liquid for surface texturing. The texturing temperature is 65°C and the texturing time is 180s.

[0095] Example 12

[0096] A. Prepare the texturing solution: take 13g xylitol, 3g polyvinyl alcohol, 5g o-methoxyphenol, 0.4g dopamine hydrochloride, 0.35g ascorbic acid, 0.15g sodium phenylacetate, 0.6g sodium isophthalate, 0.8g triethanolamine, 1.5g polypropylene glycol, 0.5g β-cyclodextrin, 2.5g Tween-20, 50g tetramethylguanidine, and 922.2g deionized water.

[0097] B. Use a vertical mixer to mix it thoroughly.

[0098] C. Texturing: Immerse the single crystal silicon wafer in the texturing liquid for surface texturing. The texturing temperature is 65°C and the texturing time is 180s.

[0099] Comparative Example 1

[0100] A. Prepare the texturing solution: take 2g dopamine hydrochloride, 0.3g isooctyl polyoxyethylene ether monophosphate, 0.3g methyl laurate ethoxylate, 0.4g methyl stearate ethoxylate, 3g erythritol, 2g xylitol, 2.5g mannitol, 2.5g sorbitol, 1g polyvinyl alcohol, 1.5g sodium formate, 30g sodium hydroxide, and 60g deionized water.

[0101] B. Use a paddle stirrer to mix thoroughly.

[0102] C. Texturing: Immerse the single crystal silicon wafer in the texturing liquid for surface texturing. The texturing temperature is 65°C and the texturing time is 180s.

[0103] Comparative Example 2

[0104] A. According to the mass percentage, 2.5% of hydrolyzed polyacrylonitrile sodium salt, 0.5% of polyaspartic acid, 0.5% of polydiaminobutyric acid, 0.05% of branched polyethyleneimine, 0.2% of dodecyltrimethylammonium chloride and 96.25% of deionized water are mixed and stirred to prepare a texturing additive;

[0105] B. Add sodium hydroxide and deionized water into the texturing tank to prepare a 1wt% alkaline solution, then add the texturing additive prepared in step A, stir evenly to prepare a texturing solution, wherein the mass ratio of the texturing additive to the alkaline solution is 0.7:100;

[0106] C. Texturing: Immerse the single crystal silicon wafer in the texturing liquid for surface texturing. The texturing temperature is 65°C and the texturing time is 180s.

[0107] After the texturing was completed, the surface performance of seven groups of solar cell monocrystalline silicon wafers was tested, and the test results are as follows:

[0108]

[0109]

[0110] It is not difficult to see from the above data that the monocrystalline silicon texturing liquid of the present invention can greatly reduce the reflectivity of the monocrystalline silicon wafer after texturing when applied to the surface texturing of monocrystalline silicon solar cells. Compared with conventional alkaline texturing liquid, the weight loss is smaller and the reflectivity is lower. At the same time, the texturing effect is good and the appearance is normal. By comparing Examples 1 and 5, it can be found that after increasing the proportion of the texturing liquid ingredients, the product effect is still good and suitable for proportional enlargement. By comparing Examples 5 and 7, it can be found that the use of different stirring equipment can change the preparation efficiency of the texturing liquid, and the uniformity of the product affects the texturing effect of the product. By comparing Examples 2 and 8, it can be found that increasing the amount of velvet modifier is beneficial to the uniformity of the pyramid on the texturing surface, thereby improving the photoelectric conversion efficiency. By comparing Examples 2 and 9, it can be found that the optimization of the defoaming agent can improve the texturing effect of the product, especially the appearance of the product. The present invention provides an efficient and environmentally friendly single crystal silicon texturing process, which realizes the uniform distribution and densification of the pyramid structure on the surface of the silicon wafer by using specific nucleating agents, defoaming agents, primary and secondary corrosion inhibitors, complexing agents, texturing modifiers and surfactants, effectively reduces the reflectivity and improves the photoelectric conversion efficiency. These additives not only optimize the texturing effect, but also reduce the use of chemicals and environmental pollution, extend the service life of the texturing solution, reduce production costs, and ensure the safety and environmental protection of the additives.

[0111] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A novel single crystal silicon texturing solution, characterized in that: The composition includes the following components in percentage by weight: 0.8% to 1.3% nucleating agent, 0.2% to 0.3% defoaming agent, 0.5% primary corrosion inhibitor, 0.03% to 0.15% secondary corrosion inhibitor, 0.05% to 0.08% complexing agent, 0.1% to 0.2% suede modifier, 0.25% surfactant, 3% to 5% organic alkali solution, and the balance is deionized water.

2. The novel single crystal silicon texturing solution according to claim 1 is characterized in that: The nucleating agent is one or more of erythrose, arabinose, glucose, fructose, galactose, sucrose, trehalose, melibiose, fucose, rhamnose, cellobiose, gentiobiose, cellotriose, gentiotriose, melezitose, raffinose, stevioside, stachyose, lactitol, maltitol, isomalt, erythritol, xylitol, mannitol and sorbitol.

3. The novel single crystal silicon texturing solution according to claim 1 is characterized in that: The defoaming agent is one or more of polyvinyl alcohol, polydimethylsiloxane, lauric acid and palmitic acid.

4. The novel single crystal silicon texturing solution according to claim 1, characterized in that: The main corrosion inhibitor is one or more of catechol, o-methoxyphenol, 2-methoxy-4-methylphenol, catecholamine and bis-catechol ligand.

5. The novel single crystal silicon texturing solution according to claim 1, characterized in that: The secondary corrosion inhibitor is one or more of dopamine hydrochloride, amine wanda, L-cysteine, ascorbic acid, acetic acid, propionic acid, benzoic acid, oxalic acid, salicylic acid, sodium silicate, sodium formate, sodium acetate, sodium lactate, sodium oxalate, sodium succinate, sodium benzoate, sodium phenylacetate, sodium isophthalate, sodium lignin sulfonate, and sodium methylene bisnaphthalene sulfonate.

6. The novel single crystal silicon texturing solution according to claim 1, characterized in that: The complexing agent is one or more of tetrasodium ethylenediaminetetraacetate, triethanolamine, sodium nitrilotriacetate, and sodium diethylenetriaminepentacarboxylate.

7. The novel single crystal silicon texturing solution according to claim 1, characterized in that: The suede modifier is one or more of polyethylene glycol, polypropylene glycol, beta-cyclodextrin, xylan, modified starch and betaine.

8. The novel single crystal silicon texturing solution according to claim 1, characterized in that: The surfactant is one or more of fatty alcohol polyoxyethylene ether AEO-7, fatty alcohol polyoxyethylene ether AEO-9, alkylphenol polyoxyethylene ether OP-10, Tween 20 and Tween 80.

9. The novel single crystal silicon texturing solution according to claim 1, characterized in that: The organic alkali solution is tetramethylguanidine.

10. A method for preparing the novel single crystal silicon texturing solution according to any one of claims 1 to 9, comprising the following steps: A. Preparation of texturing liquid: Add nucleating agent, defoaming agent, primary corrosion inhibitor, secondary corrosion inhibitor, complexing agent, suede modifier, surfactant and organic alkali solution into deionized water according to mass ratio, and stir evenly to obtain texturing liquid; B. Use a paddle stirrer, propeller stirrer, turbine stirrer, anchor stirrer, frame stirrer, ribbon stirrer, magnetic stirrer, electric heater, forced mixer, concrete mixer, vertical mixer, new mixer or homogenizing equipment to fully mix the texturing liquid; C. Texturing: Immerse the single crystal silicon wafer in the texturing liquid for surface texturing. The texturing temperature is 65°C and the texturing time is 180s.

Citation Information

Cited By

  • Texturing agent composition and texturing liquid

    CN119980479A

  • Monocrystalline silicon texturing additive, preparation method thereof and texturing liquid containing monocrystalline silicon texturing additive

    CN120758976A

  • Texturing agent composition and texturing solution

    WO2026193982A1