Bio-based polymer stock solution coloring melt spinning fiber and preparation method thereof
By mixing polylactic acid slices with color masterbatch and compatible agent before spinning, the problem of poor alkali resistance and weak high temperature resistance during the dyeing process is solved, and excellent mechanical and color properties are prepared The polylactic acid colored silk achieves more efficient dyeing effect and environmental protection.
Patent Information
- Application Number
- CN202411063312.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-08
AI Technical Summary
During the dyeing process, polylactic fiber has problems such as poor alkali resistance, weak high temperature resistance, difficulty in coloring, and poor hydrophilicity, which affects its physical and chemical properties and dyeing effect.
Using the stock liquid coloring method, the polylactic acid slices are fully mixed with the color masterbing and compatible agent before spinning, and the polylactic acid colored silk with color is prepared by melt spinning. The specific processes include drying, melt extrusion, spinning, Stretch and wind, control the amount of color masterbing added, the proportion of compatibilizer and process parameters to improve the mechanical and color properties of the fiber.
The prepared polylactic acid colored wire has good mechanical properties and excellent color properties. The blue fiber has the highest strength, the black fiber has the largest elongation, and is uniform in color and good color fastness. The production cycle is short, the cost is low and the pollution is less.
Smart Images

Figure CN118910760A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical fiber preparation, and in particular relates to a bio-based polymer solution-dyed melt-spun fiber and a preparation method thereof. Background Art
[0002] Polylactic Acid Fiber (PLA fiber) is a biodegradable synthetic fiber, and its raw material is polylactic acid (PLA). Polylactic acid is a renewable resource produced by fermentation of plant-derived materials (usually plants containing glucose such as corn or sugar cane). Not only is the raw material of polylactic acid renewable, but its products after full degradation are water and carbon dioxide, and it does not produce harmful gases after combustion, so polylactic acid fiber is an environmentally friendly and sustainable material.
[0003] However, the main challenges facing the dyeing process of PLA fibers include poor alkali resistance, poor high temperature resistance, difficulty in coloring, and poor hydrophilicity. These characteristics make the fiber vulnerable to damage during the dyeing process, affecting its physical and chemical properties and dyeing effect. Therefore, it is necessary to explore new dyeing methods and technologies to improve the dyeing efficiency, fastness and environmental protection of PLA fibers while protecting the physical properties of the fibers.
[0004] Solution dyeing, also known as pre-spinning dyeing, is a dyeing technology that directly produces colored fibers by adding appropriate colorants to the spinning solution or melt and mixing them thoroughly. This method allows coloring and spinning to be carried out simultaneously, and has the advantages of uniform coloring, good color fastness, high dye uptake, short production cycle, low cost, and less pollution. Summary of the invention
[0005] The purpose of the present invention is to solve the problem that the current polylactic acid fiber is difficult to color, and to provide a solution-dyed bio-based polymer melt-spun fiber and a preparation method thereof. The polylactic acid colored silk prepared by this method has good mechanical properties and excellent color properties, and has great application prospects as an environmentally friendly and sustainable material.
[0006] The present invention adopts the following technical solutions:
[0007] A bio-based polymer solution-dyed melt-spun fiber and a preparation method thereof, comprising:
[0008] The polylactic acid chips, masterbatch and compatibilizer are used as raw materials and prepared by melt spinning. Specifically, in the spinning process, before adding the spinning raw materials, the polylactic acid chips are dried and mixed with a certain proportion of masterbatch and compatibilizer, and then a series of spinning processes such as melt extrusion, spinning, stretching and winding are used to prepare colored polylactic acid colored yarns.
[0009] In the above technical solution, further, the coloring masterbatch is added in an amount of 0.1% to 0.5% of the mass of the dry polylactic acid chips, and the compatibilizer is added in an amount of 0.5% to 3% of the mass of the dry polylactic acid chips.
[0010] Furthermore, the melting temperature is 190° C. and the extrusion speed is 10 mm / min.
[0011] Furthermore, the stretching process is: double-roller stretching, the rotation speed of roller 1 is 150 rpm, the rotation speed of roller 2 is 225 rpm, and the fiber passes through roller 1 and roller 2 in sequence for stretching.
[0012] Furthermore, the winding process is as follows: reciprocating speed: 50 mm / min, winding speed: 300 rpm.
[0013] The polylactic acid colored yarns prepared by this method have good mechanical properties and excellent color properties. Among them, the blue polylactic acid colored yarns have the highest strength, with an average strength of 1.43 cN / dtex, and the black polylactic acid colored yarns have the highest elongation, with an average elongation of 366.12%.
[0014] The beneficial effects of the present invention are:
[0015] The present invention aims at the main challenges faced by the current polylactic acid fiber dyeing process, including poor alkali resistance, weak high temperature resistance, difficulty in coloring, poor hydrophilicity, etc. These characteristics make the fiber easily damaged during the dyeing process, affecting its physical and chemical properties and dyeing effect. The method of stock solution coloring is used to fully mix the color masterbatch with the polylactic acid slice before spinning to directly produce colored fibers. This method can make coloring and spinning proceed at the same time, and has the advantages of uniform coloring, good color fastness, high dyeing rate, short production cycle, low cost, less pollution, etc.
[0016] The invention adopts a solution coloring method to color the polylactic acid fiber to prepare polylactic acid colored yarn with excellent mechanical and color properties, which provides a new idea for the coloring of polylactic acid materials and a new reference for the application and promotion of polylactic acid materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is the polylactic acid colored yarn spun with the same content of masterbatch and different content of compatibilizer;
[0018] Figures 2 to 6 It is the polylactic acid colored yarn spun by using the same content of compatibilizer and different color masterbatches with different content of masterbatches;
[0019] Figure 7 This is a comparison chart of the stretching of polylactic acid colored yarns with different concentrations of compatibilizers;
[0020] Figure 8It is the stress-strain diagram of polylactic acid colored yarn with the same color, the same proportion of compatibilizer, and different proportions of masterbatch;
[0021] Fig. 9 This is an optical microscope image of blue polylactic acid colored silk magnified 100 times;
[0022] Fig.10 This is an optical microscope image of the pink polylactic acid colored silk magnified 100 times;
[0023] Fig.11 This is an optical microscope image of the orange polylactic acid colored silk magnified 100 times;
[0024] Fig.12 This is an optical microscope image of black polylactic acid colored silk magnified 100 times;
[0025] Fig.13 This is an optical microscope image of yellow polylactic acid colored silk magnified 100 times;
[0026] Fig.14 This is the K / S curve of blue polylactic acid colored silk before and after sun exposure;
[0027] Fig.15 This is the K / S curve of pink polylactic acid colored silk before and after sun exposure;
[0028] Fig.16 This is the K / S curve of orange polylactic acid colored silk before and after sun exposure;
[0029] Fig.17 This is the K / S curve of black polylactic acid colored silk before and after sun exposure;
[0030] Fig.18 This is the K / S curve of yellow polylactic acid colored silk before and after sun exposure;
[0031] Fig.19 This is a scanning electron microscope image of polylactic acid colored silk magnified 2000 times;
[0032] Fig. 20 This is a scanning electron microscope image of masterbatch (K7090) powder magnified 20,000 times;
[0033] Fig.21 This is an optical microscope image of blue (K7090) masterbatch powder magnified 100 times;
[0034] Fig. 22 This is an optical microscope image of pink (K4270FP) masterbatch powder magnified 100 times;
[0035] Fig.23 This is an optical microscope image of orange (red E2G) masterbatch powder magnified 100 times;
[0036] Fig.24This is an optical microscope image of black (black 2G) masterbatch powder magnified 100 times;
[0037] Fig.25 This is an optical microscope image of yellow (orange 3G) masterbatch powder magnified 100 times;
[0038] Fig.26 This is the particle size distribution curve of blue (K7090) masterbatch powder tested three times;
[0039] Fig. 27 This is the particle size distribution curve of pink (K4270FP) masterbatch powder tested three times;
[0040] Fig.28 This is the particle size distribution curve of orange (red E2G) masterbatch powder tested three times;
[0041] Fig.29 This is the particle size distribution curve of black (black 2G) masterbatch powder tested three times;
[0042] Fig.30 It is the particle size distribution curve of yellow (orange 3G) masterbatch powder tested three times. DETAILED DESCRIPTION
[0043] The present invention is further described in detail below with reference to the accompanying drawings and specific examples.
[0044] Process route: PLA slice drying and raw material preparation → melt extrusion → spinning → stretching → winding spinning operation:
[0045] (1) Pour the material into the hopper (when the equipment is working, pay attention to add granular material in time);
[0046] (2) Set the temperature and install a suitable extruder head;
[0047] (3) Wait for 5-10 minutes for the temperature to reach the set temperature, allowing the machine temperature to balance;
[0048] (4) Adjust the appropriate extrusion speed, press the start button, and start the motor to extrude the fiber;
[0049] (5) After the material is extruded, start the drafting machine and the winding machine, and use tweezers to send the fiber to the drafting roller and the winding roller;
[0050] (6) The temperature and extrusion speed can be fine-tuned during the spinning process, and the corresponding forward stretching machine speed and winding speed also need to be fine-tuned accordingly.
[0051] Polylactic acid slice drying:
[0052] The polylactic acid slices were spread flat on a tray, placed in a vacuum oven, and dried at 80°C for 24 hours.
[0053] (1) Remove moisture
[0054] Polylactic acid is polymerized from lactic acid. There are ester bonds in the polylactic acid molecule, and the ester bonds are easily hydrolyzed. Ester bond hydrolysis is the main way of polylactic acid degradation. Moreover, the hydrolysis reaction can be automatically catalyzed by the groups (—COOH) produced by hydrolysis. The ester bond hydrolysis is slow at first, but then it will accelerate. The hydrolysis reaction occurs not only on the surface of polylactic acid, but also penetrates into the entire polymer. For semi-crystalline polylactic acid, hydrolysis is divided into two stages: in the first stage, water molecules diffuse rapidly into the amorphous region, followed by hydrolysis; the second stage is the hydrolysis of the crystalline region, which is relatively slow. For polylactic acid with an amorphous structure, hydrolysis only has the first stage.
[0055] In addition, water in the melt will form bubbles during spinning, and the bubbles will be mixed in the melt stream, which is very likely to cause spinning drifting, hairy, broken, etc., and even leave hidden dangers in the monofilament, causing hairy or broken ends during post-stretching. Therefore, the slices must be dried before the high-temperature spinning process.
[0056] (2) Improve the softening point
[0057] The raw material polylactic acid chips are amorphous structures with a very low softening point. When spinning with such chips, the chips will quickly soften and become sticky after entering the screw extruder, causing "ring knots" to block and interrupt production. However, the dried chips will form partial crystals, which greatly increases the softening point. The higher the crystallinity, the higher the softening point and the harder the chips. After such chips enter the screw extruder, the "ring knot" phenomenon will be avoided.
[0058] The dried polylactic acid chips are fully mixed with a compatibilizer and masterbatch in an appropriate proportion, and then the mixture is fed into a screw extruder for melting and extrusion. In order to ensure uniform and smooth filament output and not affect the subsequent spinning process, the raw materials should be kept uniform and stable at the feeding port. Balanced and stable feeding is a key factor affecting the quality of product fibers. In addition, since the extrusion speed of polylactic acid during the spinning process is not fast, the polylactic acid raw material stays in the screw for a relatively long time, and the probability of polylactic acid degradation increases. In order to reduce the degradation of polylactic acid raw materials and thus affect the quality of spinning, high-speed discharge should be performed at regular intervals to obtain a polylactic acid melt with a relatively low degradation rate.
[0059] The melt extrusion of polylactic acid chips in the extruder is an extrusion process from solid state to high-temperature viscous flow state. The extruder must simultaneously perform the dual functions of extrusion and transportation and heating and melting. The chips move along the screw groove toward the die head, and the physical state undergoes the transformation from glassy state, high elastic state, to viscous flow state.
[0060] This experiment uses Huizhi electrospinning desktop melt spinning equipment.
[0061] Spinning:
[0062] After the melt is ejected from the spinneret into a thin stream, it gradually cools and forms along the path of the filament. The temperature, diameter, movement speed, force, viscosity and internal structure of each point on the filament are changing. External conditions have a great influence on the uniformity of the fineness, unevenness of strength and elongation and post-stretching properties of the filament.
[0063] Along the spinning direction, the cooling process of the filament can be divided into three regions: flow deformation zone, solidification deformation zone and solid state movement zone.
[0064] 1. Flow deformation zone
[0065] After the melt leaves the control of the spinneret micropores, it will expand within a distance of about 5 to 10 mm from the spinneret surface. This is due to the release of elastic deformation energy and static pressure energy generated by the sudden change in melt flow rate, which causes the diameter to expand. The expansion phenomenon is not good for spinning. It not only causes uneven filaments, but also causes adhesion to the spinneret, broken ends, and hairy filaments. If measures such as appropriately reducing the viscosity of the melt, increasing the spinning temperature, and selecting spinnerets with a larger aspect ratio are taken, the degree of expansion can be reduced.
[0066] Although the temperature has dropped in the flow deformation zone, the flow properties are very good, so it is easy to become thinner after being pulled. The resulting macromolecules have a low degree of axial arrangement and a small degree of orientation.
[0067] 2. Solidification deformation zone
[0068] The solidification deformation zone is the most important area for cooling and solidification. Under the traction of the winding mechanism and certain cooling conditions, the melt flow changes the most in this area, and changes occur in temperature, viscosity, diameter and macromolecular structure, and gradually solidifies into filaments.
[0069] (1) Diameter change. Because the winding mechanism pulling speed V (called spinning speed or winding speed) greatly exceeds the spinning speed V0 (that is, the speed at which the melt is ejected in the micropores), the filaments are stretched and thinned until the solidification point, and the diameter remains basically unchanged.
[0070] (2) Changes in melt temperature and viscosity. The melt stream is cooled by the surrounding air, and its temperature drops rapidly, while its viscosity rises quickly. When the viscosity reaches a certain value, it loses fluidity and becomes solid.
[0071] (3) Changes in the internal structure of the filaments. The internal structure of the filaments mainly includes orientation and crystallinity. Since the crystallization temperature needs to be below the melting point and above the glass transition temperature, and it takes a certain amount of time to proceed, the glass transition temperature of polylactic acid fiber is relatively high, and the temperature drops very quickly, so it has fallen below the glass transition temperature before crystallization, resulting in the internal structure of the filaments being in an amorphous (non-crystalline) state.
[0072] The degree to which the macromolecular chains are regularly arranged along the axial direction of the filament under the action of external force is called the degree of orientation, and the size of the birefringence "Δn" is used to measure the degree of orientation (a large Δn means a large degree of orientation).
[0073] 3. Solid state mobile area
[0074] From the solidification point, the filaments move at the same pulling speed, and the forming is completed. In order to reduce the temperature of the filaments when they enter the filament reel or winding mechanism, a certain cooling distance is generally required, so there is a tunnel for a distance under the filament chamber. However, when the spinning speed increases, the role of the tunnel becomes smaller.
[0075] draft:
[0076] Drafting is a process of stretching and heat setting the spun fibers, the purpose of which is to improve the quality of the fibers by changing the microstructural characteristics inside the fibers. The polylactic acid fibers are transferred from the spinneret to the drafting mechanism and the drafting process is completed by two drafting rollers.
[0077] Drawing machine: Drawing roller: double roller, circumference 20 cm, speed: 0.1-300rpm, accuracy 0.1rpm, steering: one-button adjustment of roller steering.
[0078] Winding:
[0079] The winding process is the last step in the entire production process, which is used to wind the produced fibers or yarns into rolls for storage, transportation and subsequent processing. This step is the last link in the entire production chain and is very important for ensuring product quality and facilitating subsequent processing.
[0080] Fiber winder: Collecting roller: circumference 10cm, length 10cm, rotation speed: 0.1-300rpm, precision 0.1rpm reciprocating distance: 0-15cm adjustable, reciprocating speed: 1-1000mm / min, precision 1mm / min.
[0081] Example 1
[0082] The above method was used to set the addition amount of masterbatch (K7090) to 0.1% of the mass of dry polylactic acid chips, and the addition amount of compatibilizer (polyethylene wax) to 0.5% to 3.0% of the mass of dry polylactic acid chips, for a total of six groups. Spinning temperature: 190°C, screw extrusion speed: 10mm / min, roller 1: 150rpm, roller 2: 225rpm, reciprocating speed: 50mm / min, take-up speed: 300rpm, winding time: 2min, and conduct the experiment; the obtained samples are as follows Figure 1 As shown in the figure, from left to right, the corresponding polylactic acid colored yarn samples are respectively 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, and 3.0% of the compatibilizer addition amount.
[0083] Example 2
[0084] The above method was used to set the addition amount of compatibilizer (polyethylene wax) to 3.0% of the mass of dry polylactic acid chips, the addition amount of masterbatch (in order K7090, K4270FP, red E2G, black 2G, orange 3G) to 0.1% to 0.5% of the mass of dry polylactic acid chips, and a total of 25 groups of five colors. Spinning temperature: 190°C, screw extrusion speed: 10mm / min, roller 1: 150rpm, roller 2: 225rpm, reciprocating speed: 50mm / min, take-up speed: 300rpm, winding time: 2min, and the experiment was carried out. The samples of different colors were obtained as follows Figure 2-6 As shown, from left to right in each figure, the corresponding polylactic acid colored yarn samples are respectively added with masterbatch amounts of 0.5%, 0.4%, 0.3%, 0.2%, and 0.1%.
[0085] Effects of different compatibilizers, masterbatches and color changes on the mechanical properties and color of the resulting polylactic acid colored yarns Figure 7 , Figure 8 As shown:
[0086] Different masterbatches will affect the physical and mechanical properties of solution-dyed PLA fibers. First, from the perspective of changes in the masterbatch ratio, changes in the masterbatch ratio did not have an obvious regular effect on fiber strength. However, when comparing masterbatches of different colors, it was found that the PLA fibers endowed with blue and pink masterbatches had better strength properties, while the black fibers showed better elongation. In contrast, the yellow fibers performed poorly in both strength and elongation.
[0087] In terms of color performance, the polylactic acid colored silk prepared in the experiment showed good coloring effect under naked eye observation, such as Figures 9 to 13 However, under the microscope, the blue and pink fibers have the problem of insufficient dissolution of the masterbatch, uneven size and distribution. In contrast, the other three color masterbatches (non-blue and pink) have better coloring effects in the fibers, as shown by the masterbatch being fully dissolved, the fibers being evenly colored and having good gloss.
[0088] Further analysis of the relationship between masterbatch size and fiber properties, such as Figures 21 to 30 The study found that the mechanical properties and color properties of solution-dyed polylactic acid fibers are somewhat correlated with the masterbatch particle size. This finding provides an important reference for optimizing the selection and ratio of masterbatches and improving the comprehensive performance of polylactic acid fibers.
[0089] Different colors of polylactic acid yarns have different performances in terms of light fastness, such as Figures 14 to 18 , the K / S value of some fibers decreased after sun exposure, while the K / S value of other fibers increased, especially the K / S value of a group of red fibers remained almost unchanged after sun exposure. Although the color fastness to sunlight of some fibers did not show obvious regularity, in general, the K / S value of fibers showed a downward trend after sun exposure.
[0090] The embodiments described above provide a detailed description of the preparation scheme of the present invention. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the present invention. Any modifications, supplements or similar substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing bio-based polymer solution-dyed melt-spun fibers, characterized in that: include: The polylactic acid chips, masterbatch and compatibilizer are used as raw materials and prepared by melt spinning. Specifically, in the spinning process, before adding the spinning raw materials, the polylactic acid chips are dried and mixed with a certain proportion of masterbatch and compatibilizer, and then the colored polylactic acid colored yarn is prepared according to the spinning process of melt extrusion, spinning, stretching and winding.
2. The method for preparing bio-based polymer solution-dyed melt-spun fibers according to claim 1, characterized in that: The addition amount of the masterbatch is 0.1% to 0.5% of the mass of the dry polylactic acid slices.
3. The method for preparing bio-based polymer solution-dyed melt-spun fibers according to claim 1, characterized in that: The added amount of the compatibilizer is 0.5% to 3.0% of the mass of the dry polylactic acid slices.
4. The method for preparing bio-based polymer solution-dyed melt-spun fibers according to claim 1, characterized in that: The melting temperature is 190° C. and the extrusion speed is 10 mm / min.
5. The method for preparing bio-based polymer solution-dyed melt-spun fibers according to claim 1, characterized in that: The stretching process is: double-roller stretching, the rotation speed of roller 1 is 150 rpm, and the rotation speed of roller 2 is 225 rpm.
6. The method for preparing bio-based polymer solution-dyed melt-spun fibers according to claim 1, characterized in that: The winding process is as follows: reciprocating speed: 50 mm / min, winding speed: 300 rpm.
7. A bio-based polymer solution-dyed melt-spun fiber, characterized in that: The fiber is prepared by the method according to any one of claims 1 to 6, and the fiber linear density is 26 to 41 dtex.
8. The bio-based polymer solution-dyed melt-spun fiber according to claim 7, characterized in that: The average strength of the fibers is 1.43 cN / dtex.
9. The bio-based polymer solution-dyed melt-spun fiber according to claim 7, characterized in that: The average elongation of the fibers is 366.12%.
Citation Information
Patent Citations
Polylactic acid fiber color silk
CN108048924A
Stock-solution-coloring high-melting-point polylactic acid fibers and preparation method thereof
CN108070914A
Stock solution-colored polylactic acid fiber and preparation method thereof
CN108193316A
Preparation method for polylactic acid plant dye color master batch
WO2023020338A1
Cited By
Method for improving irregularity of bio-based polymer melt spinning fibers