Method for preparing boron nitride continuous fiber through aldehyde-cyano guanidine-boron oxygen resin filamentation
Boron nitride continuous fibers were prepared by a low-crosslinking liquid aldehyde-cyanoguanidine-boroxy resin filamentation method, which solved the problems of convenience, safety and economy in the preparation of high-performance boron nitride continuous fibers in the existing technology, and realized the production of high-strength, low-porosity boron nitride continuous fibers.
Patent Information
- Application Number
- CN202411123875.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-08
AI Technical Summary
Existing technologies are difficult to use conveniently, safely, and economically to prepare high-performance boron nitride continuous fibers, and they also have problems such as high energy consumption, high safety risks, and poor fiber mechanical properties during the high-temperature melting process.
Boron nitride continuous fibers are prepared by using a low-crosslinked liquid aldehyde-cyanoguanidine-boroxy resin spinning method, which involves molding, heat treatment and high-temperature pyrolysis of the low-crosslinked liquid resin. This avoids high-temperature melting and ammonia treatment, and utilizes a nitrogen protective atmosphere for high-temperature conversion.
It achieves low cost, high safety, simplified process steps, improved fiber strength and reduced porosity defects, reduced production energy consumption, and is suitable for large-scale production.
Smart Images

Figure CN118910767A_ABST
Abstract
Description
Technical field:
[0001] The invention relates to the technical field of advanced synthesis of high-end ceramic fibers, and in particular to a method for preparing boron nitride continuous fibers by filamentation of aldehyde-cyanoguanidine-boryl resin. Background technology:
[0002] Hexagonal boron nitride (h-BN) is a ceramic material with excellent properties such as high temperature stability, high chemical inertness and high thermal conductivity, and therefore has broad application prospects in many fields. As a very important special form of h-BN, h-BN continuous fiber shows important application value in extreme environments such as high temperature and high strength. With its excellent performance, h-BN continuous fiber has broad application potential in aerospace, high temperature materials, thermal management and high-end composites. However, the current convenient and efficient preparation technology is still the main limiting factor for its widespread application.
[0003] The preparation of h-BN continuous fibers is one of the keys to h-BN material research. The basic method is to first prepare continuous precursor fibers and then convert them into boron nitride continuous fibers at high temperatures. The main preparation methods include melt spinning, electrospinning and spin spinning, and the specific selection depends on the type and properties of the precursor. The high-temperature conversion process, including polymerization, pyrolysis and high-temperature nitridation, determines the quality of boron nitride continuous fibers.
[0004] The raw materials and high temperature treatment process of the precursor for preparing boron nitride continuous fibers are mainly divided into four categories:
[0005] The first category is organic boron compounds or polymers containing boron-nitrogen bonds: including cyclic boron nitrogen, polycyclic boron nitrogen, borazane or polyborazane (related patents: US6774074B2 and US6967179B2, etc.). These precursors require expensive, highly active and highly toxic gas-phase boron halides or boranes as precursor synthesis raw materials. These raw materials are extremely sensitive to humidity and temperature, and there are high safety risks in synthesis and storage.
[0006] The second category, inorganic boron oxide, boric acid or borate: This filamentation process requires melting the raw materials at a high temperature of about 1000°C, and then filamenting the high-temperature melt into a precursor of boron oxide continuous fiber (related patents: US3620780, CN107540382B and US3668059A, etc.). This high-temperature filamentation operation consumes a lot of energy and has a high risk of high temperature danger.
[0007] The third category is the combination of boron oxide compounds and high molecular polymers: the boron oxide components are spun and combined into polymer continuous fibers, and then these additional polymer components are removed by high temperature decarbonization and debinding, and finally the remaining boron oxide components are nitrided to convert into boron nitride continuous fibers (related patents: CN101428813B, CN101254904B; related literature: Nanotechnology 2009, 20, 345603). The high temperature nitridation conversion must use ammonia for decarbonization and debinding, which easily leads to the formation of macroporous defects in the fiber, and the fiber mechanical properties are poor.
[0008] The fourth category is a combination of boron nitride precursor and high molecular polymer: similar to the third category, it is produced by electrospinning, but the same high-temperature ammonia nitridation process also causes a large number of macroporous defects to form inside the fiber, and the mechanical properties of the obtained fiber are also poor.
[0009] In view of the above preparation methods, in order to meet the needs of modern industry and high-end technology, it is particularly important to develop a convenient, safe and economical new raw material for filamentation and to prepare boron nitride continuous fibers with high performance properties (high strength and low porosity defect fibers). Summary of the invention:
[0010] The purpose of the present invention is to provide a method for preparing boron nitride continuous fibers by filamenting an aldehyde-cyanoguanidine-boryl resin. The method utilizes the low-crosslinked liquid aldehyde-cyanoguanidine-boryl resin's low cost, low toxicity, high safety and high stability, as well as its universal and wide filamenting properties to improve the simplicity and safety reliability of its filamenting process.
[0011] The technical solutions adopted to achieve the purpose of the present invention are as follows:
[0012] In a first aspect, the present invention provides a method for preparing boron nitride continuous fibers by filamenting an aldehyde-cyanoguanidine-boryl resin, comprising the following steps:
[0013] (1) Low cross-linked liquid resin: A solution of an aldehyde-containing organic compound, cyanoguanidine and a boron-oxygen-containing compound are mixed and reacted under heating or room temperature to obtain a low cross-linked liquid resin that can remain in a spinnable liquid state without solidifying after being sealed and left to stand at a temperature not higher than 100° C. for at least two days;
[0014] Wherein, the ratio of the mass of cyanoguanidine to the mass of the boron-oxygen compound is 1.36 to 1.95;
[0015] (2) Low-crosslinked quasi-solid resin continuous fiber: The liquid resin is subjected to a filament forming process at a temperature of less than 200° C. to obtain a low-crosslinked quasi-solid resin continuous fiber;
[0016] (3) Highly cross-linked solid resin continuous fibers: low-cross-linked quasi-solid resin continuous fibers are subjected to a long-term heat treatment transformation at a target temperature in the temperature range of 70-350°C to obtain dry, fully cross-linked, highly cross-linked solid resin continuous fibers, during which no bubbling occurs;
[0017] (4) High-temperature pyrolysis reaction process: The highly cross-linked solid resin continuous fiber is directly subjected to high-temperature pyrolysis under a protective atmosphere to obtain a boron nitride continuous fiber.
[0018] In step (1) of the present invention, the liquid resin with a low degree of cross-linking can still maintain a viscosity range of 10 mPa·S-10000 mPa·S after being sealed and stored for a long time for 2-100 days in a temperature range of 25°C-84°C.
[0019] In step (1) of the present invention, at least one auxiliary nitrogen source selected from aminoguanidine, chlorfenapyr or guanidine carbonate is added to cyanoguanidine, and the amount of the auxiliary nitrogen source added is 0wt.%-10wt.% of the mass of cyanoguanidine. At this time, a cross-linking inhibitor is added to the solution containing the aldehyde-based organic matter, and the cross-linking inhibitor is 6%-30% of the mass of the solvent in the solution;
[0020] Wherein, the solution containing aldehyde-based organic matter is a solution formed by dissolving formaldehyde or acetaldehyde in a solvent;
[0021] Wherein, the solvent is a pure water solvent or a mixed solvent formed by water and a cross-linking inhibitor;
[0022] The content of formaldehyde or acetaldehyde in the solution containing aldehyde-based organic matter is in the range of 10 wt.% to 40 wt.%.
[0023] The ratio of the mass of cyanoguanidine (in grams) to the volume of the solution containing the aldehyde-based organic matter (in milliliters) in step (1) of the present invention is 0.7 to 1.6.
[0024] The boron-oxygen compound described in step (1) of the present invention is at least one of boron trioxide, boric acid or borax.
[0025] The cross-linking inhibitor described in the present invention is at least one of methylamine solution (30-40wt.%), ethylene glycolamine, monoethanolamine, N-methylethanolamine, hexamethylenetetramine, hydrochloric acid (10wt.%-37wt.%), formic acid or acetic acid.
[0026] In step (2) of the present invention, the filament forming process is to form the liquid resin into a continuous fiber of a low-crosslinked quasi-solid resin through a filament forming technology including electrospinning, centrifugal spinning, disc spinning or mechanical drawing;
[0027] Among them, the voltage of electrospinning is 10-30 kV, and the fan blowing temperature ranges from 25-70°C during the spinning process;
[0028] The centrifugal spinning speed is 1000-8000r / min, and the blast temperature in the centrifugal spinning collection chamber is in the range of 100-200°C;
[0029] The rotating disk speed of the disc spinning is 2000-10000r / min, and the temperature range of the blowing air flow provided in the disc spinning collection space is 50-100℃;
[0030] Among them, the temperature range of mechanical wire drawing is 25-35℃.
[0031] In step (3) of the present invention, the heating rate during the process of converting the low-crosslinked quasi-solid resin fiber into the highly crosslinked solid resin fiber after a long period of heat treatment under normal pressure air environment is not higher than 5°C / min, and the low-crosslinked quasi-solid resin fiber is exposed in a heating-drying device purged with a hot air flow, and the fiber formed after the high crosslinking conversion is completed does not contain any water molecule components, and any water molecule components include bound water, free water and water products;
[0032] In step (4) of the present invention, the heating / cooling rate during high-temperature pyrolysis is 5-100°C / min, the protective atmosphere is high-purity nitrogen or nitrogen, ammonia, or a mixture of ammonia and nitrogen with a volume content of less than or equal to 1% in air, and the gas flow rate is 10-1000ml / min;
[0033] The high temperature pyrolysis temperature is 1500-1800°C, the pyrolysis time is 0.5-24 hours, and the pyrolysis atmosphere is nitrogen, high-purity nitrogen, or ammonia-nitrogen mixed gas with an ammonia volume content of less than 10%;
[0034] Alternatively, the high-temperature pyrolysis is carried out in two stages, the first stage pyrolysis temperature is 1100-1400°C, the protective atmosphere is ammonia or a mixture of ammonia and nitrogen, the second stage pyrolysis temperature is 1600-1800°C, the protective atmosphere is nitrogen, and the total pyrolysis time is 0.5-24 hours.
[0035] In a second aspect, the present invention provides a boron nitride continuous fiber obtained by the above method, wherein the diameter distribution range of the boron nitride continuous fiber extends from the nanometer level to the micrometer level. When the high-temperature pyrolysis target temperature is not less than 1600°C, the specific surface area of the boron nitride continuous fiber is relatively low, ranging from 1 to 20 m 2 / g range, the tensile strength of the boron nitride continuous fiber is not less than 800MPa.
[0036] In a third aspect, the present invention also provides a product of boron nitride continuous fibers, wherein the boron nitride continuous fibers are made into boron nitride fiber felt, boron nitride fiber film, boron nitride fiber paper, boron nitride fiber cloth, boron nitride fiber block foam, and boron nitride fiber reinforced ceramic-based, polymer-based or metal-based composite materials, etc.
[0037] Compared with the existing boron nitride continuous fiber technology, the beneficial effects of the present invention are:
[0038] The method provided by the present invention has obvious advantages in terms of raw material cost, safety and simplified preparation. Compared with organic boron compounds as raw materials for filament formation, the resin spinning solution of the present invention exhibits higher chemical inertness and temperature stability to temperature and humidity. Its ultra-high thermal and humidity stability ensures high safety in the filament formation process, without the need for the inert high-temperature melting environment or the complex, multi-step synthesis, pre-melting or dissolution process required by organic boron compounds. The synthesis of the resin of the present invention is simple and has outstanding stability. It can be stored for a long time and can be used at any time, unlike the high toxicity of organic boron compound raw materials, which requires strict protective measures and anti-toxic facilities.
[0039] Compared with the method of preparing boron nitride continuous fibers by melt spinning of materials such as boron oxide and then gradually nitriding, the method provided by the present invention has the following obvious advantages. First, melt spinning of boron oxide and other boron-oxygen-containing compounds requires melting these compounds into liquid melts in a high-temperature environment exceeding 1000°C. Such high-temperature melting equipment has high energy consumption, and there is a high risk of high-temperature radiation and fire in the filamentation process of the high-temperature liquid melt. In contrast, the temperature and conditions of the low-crosslinked liquid resin prepared by the present invention are very mild, and the equipment used is the simplest and cheapest in the industry, without the need for special design and modification. In addition, the high-temperature pyrolysis process of the present invention can use only nitrogen as the protective atmosphere, which is more economical than the condition of high-temperature nitridation using ammonia.
[0040] The method provided by the present invention has obvious advantages over the method of combining a boron oxide compound and a high molecular polymer and a boron nitride precursor and a high molecular polymer. First, the solution formed by the boron oxide compound and the boron nitride precursor in these two methods is not spinnable in itself. It mainly relies on a soluble and spinnable polymer solution, and the boron oxide component or the boron nitride precursor is combined with the polymer high molecular fiber structure formed by spinning during the spinning to polymer filamentation process, forming a polymer high molecular continuous fiber as a support or fiber template, and the boron oxide component or the boron nitride precursor is uniformly mixed or loaded into these high molecular fibers to form a precursor of continuous fibers. Subsequently, this polymer fiber frame template must be removed through a high-temperature decarbonization or debinding process with an ammonia atmosphere, and then the remaining boron oxide or boron oxide nitrogen-containing macroporous fragile fibers are further high-temperature nitrided to be converted into boron nitride continuous fibers. The carbon removal and debinding process will form a large number of mesopores and larger pore structures in the fiber in situ, so that the obtained boron nitride continuous fiber has a large number of defects and pores. These defects cannot be effectively eliminated by increasing the treatment temperature, resulting in poor mechanical properties of the fiber. In contrast: the high-temperature process of step (4) of the method of the present invention does not require additional carbon removal and debinding treatment processes, and the high-crosslinked resin continuous fiber obtained in step (3) can be directly subjected to pyrolysis treatment under a high-temperature nitrogen environment to obtain a high-quality boron nitride continuous fiber; in addition, the crosslinked solid resin continuous fiber prepared by the present invention has a high degree of crosslinking polymerization reaction in step (3), so that the resin fiber has an overall uniform crosslinking state and a certain amount of BN bonds are formed. It is not easy to produce a large pore structure during the high-temperature pyrolysis process, so that the rearrangement effect of atoms and molecules is more obvious, which promotes a significant improvement in the degree of densification inside the fiber, not only maintaining a good fiber morphology, but also having high mechanical properties and well-developed low porosity.
[0041] In general, compared with the prior art, the method for preparing continuous boron nitride fibers provided by the present invention has significant advantages in improving fiber strength, reducing fiber macropore defects, simplifying process steps and improving safety. The method not only significantly reduces production energy consumption, but also has the potential to achieve large-scale production. Therefore, the method of the present invention has broad prospects and large market potential in industrial applications. Description of the drawings:
[0042] In order to more clearly introduce the technical solutions and product types of the present invention, the drawings required for use in the description of the embodiments are briefly elaborated and illustrated below. It should be emphasized that these illustration examples are only part of the embodiments of the present invention. For ordinary technicians in this field, without paying creative work, these are likely to extend and multiply to other similar and related illustration examples. In the event that similar and similar illustrations are used as new creative embodiments, they are deemed to be infringements of the present invention.
[0043] Figure 1 A block flow chart of the steps of the method of the present invention;
[0044] Figure 2 This is a picture of an actual optical photograph of a precursor of highly cross-linked resin continuous fibers obtained in Example 1 of the present invention;
[0045] Figure 3 This is a picture of the optical photographs of the boron nitride block foam material constructed of boron nitride continuous fibers obtained in Example 1 of the present invention before and after high temperature treatment;
[0046] Figure 4 The XRD diffraction pattern of the precursor of the solid resin continuous fiber with a high degree of cross-linking obtained in Example 1 of the present invention;
[0047] Figure 5 The XRD diffraction pattern of the boron nitride continuous fiber obtained by pyrolysis treatment at 1500° C. in a nitrogen atmosphere in Example 1 of the present invention;
[0048] Figure 6 This is a comparison diagram of the XRD diffraction patterns of the boron nitride continuous fiber obtained at 1600° C. in Example 1 of the present invention and the sample pretreated with ammonia;
[0049] Figure 7 The Fourier transform infrared (FTIR) spectrum of the highly cross-linked resin continuous fiber and the boron nitride continuous fiber product obtained by direct pyrolysis at 1600° C. in Example 1 of the present invention;
[0050] Figure 8 This is a SEM image of the boron nitride continuous fiber obtained by direct pyrolysis at 1600° C. in Example 1 of the present invention;
[0051] Fig. 9 The boron nitride continuous fibers ( Fig. 9 Figures b, c and d in Figure 2) are compared with those that require pre-treatment with ammonia pyrolysis ( Fig. 9 (a) SEM image of the obtained boron nitride continuous fiber;
[0052] Fig.10 The figures are photos of SEM images obtained by scanning the fracture morphology of boron nitride continuous fibers under different pyrolysis conditions, wherein figure a is a SEM image of the fracture cross section of boron nitride continuous fibers obtained by pyrolysis in ammonia at 1100°C; figure b is a SEM image of the fracture cross section of the paralleled fibers obtained by ammonia pre-pyrolysis and 1600°C nitrogen treatment; figures c and d are SEM images of the fracture of boron nitride continuous fibers directly obtained by pyrolysis in a high-purity nitrogen atmosphere at 1500°C and 1600°C according to the present invention;
[0053] Fig.11 The nitrogen adsorption / desorption curve, BET specific surface area data, and pore distribution diagram of the boron nitride continuous fiber obtained by direct pyrolysis at 1500° C. in Example 1 of the present invention;
[0054] Fig.12 The figure is a comparison of the dot-line graph and statistical summary of the five-point BET test data of the boron nitride continuous fiber directly obtained at 1600° C. in Example 1 of the present invention and the boron nitride continuous fiber sample obtained by pretreatment;
[0055] Fig.13 The real-time in-situ tensile image and the real-time stress-strain curve of the tensile fracture strength test of the boron nitride continuous fiber directly obtained at 1600°C in Example 1 of the present invention are shown, wherein Figure a is the image before the tensile test, Figure b is the image after the tensile fracture, and Figure c is the relationship between the tensile strain and the load force;
[0056] Fig.14 This is an optical photograph of the oriented highly cross-linked resin continuous fiber obtained in Example 2 of the present invention and the actual fiber after pyrolysis;
[0057] Fig.15 This is a photo of the SEM image of the boron nitride continuous fiber obtained by direct pyrolysis at 1600° C. in Example 2 of the present invention;
[0058] Fig.16 The figure is a comparison of the dot-line graph and statistical summary of the five-point BET test data of the boron nitride continuous fiber obtained by direct pyrolysis at 1600° C. in Example 2 of the present invention and the boron nitride continuous fiber sample obtained by pretreatment;
[0059] Fig.17 This is a photograph of a SEM image of a boron nitride continuous fiber product with oriented arrangement obtained directly at 1600° C. in Example 2 of the present invention;
[0060] Fig.18 TEM image comparison of the boron nitride continuous fiber obtained by direct 1600°C pyrolysis in Example 2 of the present invention and the boron nitride continuous fiber sample obtained by pretreatment; Figure a is a TEM image of the boron nitride continuous fiber sample obtained by pretreatment, that is, a TEM image of the boron nitride continuous fiber obtained by pretreatment in ammonia at 1100°C and then in a nitrogen environment at 1600°C; Figure b is a TEM image of the direct nitrogen 1600°C pyrolysis product of Example 2;
[0061] Fig.19 This is a comparison photograph of the optical objects of the highly cross-linked solid resin continuous fiber in Example 3 of the present invention and the coarse boron nitride continuous fiber obtained by direct pyrolysis at 1600°C. Specific implementation method:
[0062] In order to better help technical professionals in the field understand the present invention, the details of the present invention will be further described in detail below in conjunction with embodiments and the method mechanism of the present invention will be further analyzed and explained. It should be emphasized that the following examples are only used to more clearly illustrate the present invention and should not be construed as any limitation to the scope of protection of the present invention. Professionals in the technical field can make various improvements and adjustments based on the content of the present invention, and these improvements and adjustments still belong to the protection category of the present invention.
[0063] Unless otherwise defined, the professional terms used in the present invention are consistent with the meanings commonly understood by those skilled in the art. Various raw materials, reagents, instruments, equipment and some consumable materials used in the present invention can be purchased from the market or can be prepared by existing methods.
[0064] The present invention is a method for preparing boron nitride continuous fiber by filamenting aldehyde-cyanoguanidine-boryl resin. The process flow can refer to Figure 1 , which includes the following four steps that need to be explained in detail:
[0065] Step (1) low cross-linked liquid resin: a solution of an aldehyde-containing organic compound, cyanoguanidine and a boron-oxygen-containing compound are mixed uniformly under heating or at room temperature to obtain a low cross-linked liquid resin that can remain in a spinnable liquid state without solidifying after being sealed and left to stand at a temperature not higher than 100° C. for at least two days;
[0066] The ratio of the mass of cyanoguanidine (in grams) to the volume of the solution containing the aldehyde organic compound (in milliliters) is in the range of 0.7 to 1.6.
[0067] The value of the ratio of the mass (in grams) of cyanoguanidine to the mass (in grams) of the boron-oxygen-containing compound is in the range of 1.36 to 1.95.
[0068] The solution of the aldehyde-containing organic matter, cyanoguanidine and the boron-oxygen-containing compound are subjected to a chemical reaction in the above proportions at a temperature range of 25-84° C. with uniform stirring for 0.5 to 72 hours to obtain a liquid resin with a low degree of crosslinking.
[0069] The boron-oxygen compound satisfies the condition that it can provide sufficient HO-B-OH group components after being dissolved in an aqueous solvent or a solvent mainly composed of water. The boron-oxygen compound that can form a sufficient amount of HO-B-OH components in an aqueous solution is but not limited to at least one of boron trioxide, boric acid, or borax, preferably boric acid and borax.
[0070] The solution containing aldehyde-based organic matter is a formaldehyde aqueous solution or an acetaldehyde aqueous solution formed by dissolving formaldehyde or acetaldehyde in water; or a mixed solution of formaldehyde or acetaldehyde formed by dissolving formaldehyde in a mixed solvent mainly composed of water; the mixed solvent mainly composed of water is formed by pure water and a cross-linking inhibitor, and the weight proportion of water in the mixed solvent ranges from 70wt.% to 94wt.%.
[0071] The cross-linking inhibitor is a chain terminator when the components in the resin are about to undergo a high cross-linking polymerization reaction, including but not limited to at least one of methylamine solution (30-40wt.%), ethylene glycolamine, monoethanolamine, N-methylethanolamine, hexamethylenetetramine, hydrochloric acid (10wt.%-37wt.%), formic acid or acetic acid;
[0072] The content of formaldehyde or acetaldehyde in the solution containing aldehyde-based organic matter is in the range of 10% to 40%.
[0073] In fact, in the present invention, at least one auxiliary nitrogen source selected from aminoguanidine, herbicide or guanidine carbonate is added to cyanoguanidine, and the amount of the auxiliary nitrogen source added is 0wt.%-10wt.% of the mass of cyanoguanidine. Auxiliary nitrogen sources such as aminoguanidine, herbicide or guanidine carbonate have the effect of inducing the development of low crosslinking to high crosslinking, that is, inducing rapid high crosslinking state and causing rapid solidification of liquid state, thereby causing the resin to not have the property of being able to form a filament. Therefore, it is necessary to add corresponding crosslinking inhibitors when adding these auxiliary nitrogen sources: for example, when aminoguanidine or guanidine carbonate is used as an auxiliary nitrogen source, it can be accompanied by salts. The addition of a cross-linking inhibitor selected from one of acid (10wt.%-37wt.%), formic acid or acetic acid, or any combination of several thereof, can reduce the occurrence of rapid high-density cross-linking curing caused by the addition of aminoguanidine or guanidine carbonate, so that the liquid resin still maintains good viscosity and low cross-linking spinnability; for example, when chlorpyrifos is added as an auxiliary nitrogen source, it can be accompanied by the addition of a cross-linking inhibitor selected from one of methylamine solution (30-40wt.%), ethylene glycolamine, monoethanolamine, N-methylethanolamine or hexamethylenetetramine, or any combination of several thereof, so that the resin maintains low cross-linking and good viscosity spinnability.
[0074] Without considering the reaction inhibition between the crosslinking agent and these partially substituted reagents, and only considering the aldehyde group, cyanoguanidine and borane components, the formation reaction mechanism of the low crosslinked liquid resin in step (1) of the present invention is: assuming that cyanoguanidine is R-NH2 and the aldehyde group-containing organic matter (compound) is R-CHO, the condensation reaction between the two occurs, that is, the nitrogen atom in the amino group (-NH2) carries a lone pair of electrons and can act as a nucleophilic reagent to attack the carbon atom in the aldehyde group (-CHO) to form an unstable combination, which loses a molecule of water to form an imine bond (C=N), generating a polyimine bond intermediate (RN=CH-R') and water (H2O). The reaction equation can be written as: Subsequently, the intermediate containing polyimide bonds reacts with boric acid, i.e., the condensation product RN=CH-R' undergoes an esterification reaction with the hydroxyl group in HO-B-OH (or B(OH)3), forming a cross-linked structure connected by BO bridge bonds, forming a preliminary low-cross-linked network structure, wherein the low-cross-linked liquid resin generated during the reaction is RN=CH-R'-BOR"-N=CH-R' and water (H2O), i.e., the reaction that occurs is: RN=CH-R'+B(OH)3→RN=CH-R'-BOR"-N=CH-R'+H2O. Since the reaction temperature is concentrated in the relatively mild temperature range of 25-84°C, the resin in this state forms a small amount of slightly polymerized segments and contains a large amount of components that do not participate in the polymerization, forming a liquid resin with a certain viscosity range and a relatively stable cross-linking degree in the range of 25-84°C, which has spinnability and processability.
[0075] Liquid resins with a low degree of cross-linking can still maintain a viscosity range of 10mPa·S-10000mPa·S after long-term sealed storage for 2-100 days in a temperature range of 25°C-84°C.
[0076] Step (2) low-crosslinked quasi-solid resin continuous fibers: the liquid resin obtained in step (1) is subjected to a filament forming process at a temperature of less than 200° C. to obtain low-crosslinked quasi-solid resin continuous fibers;
[0077] The liquid resin with low cross-linking degree has a spinnable viscosity and is formed into a fiber shape by a filament forming process within a certain temperature range, at which time a quasi-solid fiber containing a trace amount of solvent components is formed;
[0078] Thanks to the key low cross-linking effect of the special nitrogen source of cyanoguanidine in the middle stage of the aldehyde-amino-boroxy resin, the resin system can maintain a high liquid state and fluidity for a long time, that is, the viscosity value ranges from 10mPa·S to 10000mPa·S, making it possible to achieve a continuous filament molding process in the temperature range of room temperature (25°C) to 200°C.
[0079] Among them, the filament forming process is to form the liquid resin into the form of continuous fibers of quasi-solid low-cross-linked resin through filament forming technologies such as electrospinning, centrifugal spinning, disc spinning or mechanical drawing; the voltage of electrospinning is selected to be 10-30 kV, and the fan blowing temperature range during the electrospinning process is 25-70°C; the centrifugal speed of centrifugal spinning is selected to be 1000-8000r / min, and the centrifugal spinning cavity blast temperature range is 100-200°C; the turntable speed of disc spinning is selected to be 2000-10000r / min, and the blowing air flow temperature range given by disc spinning is 50-100°C; the temperature range of mechanical drawing to form low-cross-linked quasi-solid resin continuous fibers is selected to be within the lower range of 25-35°C.
[0080] The quasi-solid fiber is a fiber state close to a solid state in which the low-crosslinked resin contains a small amount of solution components and is in a hydrogel-like state with low fluidity.
[0081] Step (3) high cross-linked solid resin continuous fibers: heat-treating the low cross-linked quasi-solid resin continuous fibers at a target temperature in the temperature range of 70-350° C. to obtain dry fully cross-linked high cross-linked solid resin continuous fibers, during which no bubbling occurs;
[0082] The heat treatment environment is preferably an air normal pressure environment, and the low cross-linked resin continuous fibers are heat treated in a temperature range of 70-350° C. for 24-96 hours to obtain highly cross-linked (completely cross-linked) solid resin continuous fibers.
[0083] The formation mechanism of slowly increasing the surface temperature of low-crosslinked quasi-solid resin fibers and using hot air to blow over their surfaces to transform them into highly crosslinked solid resin fibers is analyzed as follows. Under the condition of heated air purge, each monomer RN=CH-R'-BOR"-N=CH-R' in the low cross-linked resin will further cross-link to form a high cross-linked structure through the following process: the residual amino and aldehyde groups in each monomer will react with the reaction sites of the adjacent monomers to generate more imine bonds (RN=CH-R'), that is, the following reaction will occur again: R-NH2+R'-COH→RN=CH-R'+H2O; boric acid reacts with the imine intermediate to form a new boron oxygen bridge bond (BO), so that the monomers are connected to each other through the boron oxygen bridge bond, that is, the reaction will occur again: RN=CH-R'+B(OH)3→RN=CH-R'-BOR"-N=CH-R'+H2O; through multiple cross-linking reactions, multiple monomers are connected together, so that each monomer is connected to the adjacent monomer RN=CH-R'-BOR"-N=CH-R' through the boron oxygen bridge bond and the imine bond, forming a stable high cross-linked [RN=CH-R'-BOR"-N=CH-R'] n Solid resin with three-dimensional network structure. The high cross-linking reaction equation is:
[0084]
[0085] During the high cross-linking transition, the characteristic of slowly generating a large amount of water requires that the fiber be exposed to a hot air flow for rapid separation from the fiber body, thereby promoting the rapid diffusion and escape of the internally generated water molecules and further separation from the fiber surface.
[0086] Among them, the heating rate of the heat treatment of the quasi-solid low-crosslinked fibers obtained by different spinning processes should not be too high to prevent the excessively high heating rate from causing the uncrosslinked active ingredients to decompose and damage the fiber structure; or the heating is too fast to cause the high crosslinking reaction to occur too quickly, and a large number of water molecules are not able to escape from the fiber in time, which will induce bubbling behavior inside the fiber and cause damage to the fiber structure; if the escaped water on the fiber surface is not taken away in time by the hot air flow, the adjacent fiber surfaces will be fused and connected. As the high crosslinking reaction continues, the connected fibers will eventually be twisted (see Appendix). Fig.10 The obtained boron nitride continuous fibers shown in Figures a and b in the figure have undergone the phenomenon of yarn doubling); in addition, when the hot air flow is blown onto the surface of the low-crosslinked fiber, it can promptly take away the moisture generated by the further crosslinking reaction, so that the moisture does not have enough residence time to dissolve and corrode the fiber surface, inducing the deterioration of the exposed surface components that have not undergone crosslinking, thereby effectively protecting the fiber surface from damage.
[0087] Therefore, the heating rate during the high cross-linking reaction transformation process at this stage should not be too high, generally not higher than 5°C / min, and the maintenance time is relatively long, up to 96 hours.
[0088] It is worth noting that a certain amount of BN bonds can be proved to be formed in the highly cross-linked solid resin fibers. These BN bonds previously formed in the precursor (such as Figure 7 The highly cross-linked filament precursor shown is located at 782 cm -1 The typical BN vibration peak at ) plays a key role in maintaining good fiber structure invariance and improving fiber mechanical strength during the subsequent high-temperature pyrolysis process of highly cross-linked resin fibers.
[0089] In summary, the high cross-linked resin fiber obtained in step (3) must control the rate and progress of the high cross-linking reaction, and prevent bubbling, rupture, severe twisting and surface damage during the transformation of the fiber structure from the quasi-solid state to the solid state. At the same time, a certain amount of BN bonds formed during the high cross-linking process can ensure the high invariance and high mechanical strength characteristics of the fiber morphology and structure during the subsequent high-temperature pyrolysis process. Because the main by-product of the high cross-linking process is water molecules, the standard for judging whether the high cross-linking has occurred completely is to form a dry substance and no water molecules escape from the fiber. If there is no high cross-linking transformation step, this low cross-linked quasi-solid fiber will obtain a non-fiber morphology with damaged structure after direct high-temperature pyrolysis.
[0090] Step (4) high temperature pyrolysis reaction process: directly subjecting the highly cross-linked solid resin continuous fibers to high temperature pyrolysis under a protective atmosphere to obtain boron nitride continuous fibers.
[0091] The highly cross-linked solid resin continuous fiber is directly subjected to a pyrolysis reaction in a nitrogen protective atmosphere within a temperature range of 1500-1800°C for 0.5-24 hours to be converted into a boron nitride continuous fiber; wherein the heating / cooling rate is 5-100°C / min, and the air flow rate is 10-1000ml / min.
[0092] Benefited from the formation of highly cross-linked [RN=CH-R'-BOR"-N=CH-R'] n Solid resin fiber. The highly cross-linked structure contains a large number of boron oxygen (BO) bridge bonds and a certain amount of BN bonds, which makes the highly cross-linked resin continuous fiber precursor have good strength and structural stability (see Appendix Fig.14The highly cross-linked fibers electrospun as shown have certain good mechanical properties), so that there is no uncross-linked monomer or component in the further high-temperature process to undergo low-temperature pyrolysis, which leads to the collapse of the fiber structure and the rupture of the bubbles. The reaction mechanism of the pyrolysis under high-temperature nitrogen is a high-temperature pyrolysis reaction process in which the highly cross-linked resin can be converted into boron nitride (BN) under a high-temperature nitrogen environment. This process mainly involves pyrolysis and the in-situ nitridation reaction process accompanying the pyrolysis process: under nitrogen in the high temperature range of 1500-1800°C, the organic groups (R, R' and R") in the highly cross-linked resin will decompose to generate small molecular waste gas containing hydrogen, carbon, nitrogen and oxygen, which will be separated from the fiber structure. At the same time, the BO bond will be nitrided to BN bond by the nitrogen-containing component in the pyrolysis byproduct or the in-situ nitrogen-containing active site in the fiber. The formed BN bond will prompt the newly formed BN component around to rearrange and grow with itself as the connection node, thereby continuously forming the phase component of boron nitride (BN), thereby forming a fiber with a BN phase with unchanged fiber morphology and a microstructure. The overall reaction equation can be written as: or
[0093]
[0094] Benefiting from the complete cross-linking state inside the resin fiber after the high cross-linking polymerization in step (3), the high cross-linking resin fiber has a more uniform and complete three-dimensional high-density polymer connection network. The internal high cross-linking polymerization state makes the fiber uniformly transformed during the high-temperature pyrolysis to boron nitride without forming a larger pore structure. In fact, uniform micropores (less than 2nm, see the pore analysis results of the fiber obtained at 1500°C, attached) are formed inside the high cross-linking fiber during the high-temperature pyrolysis. Fig.11 ).
[0095] Different from the previous fiber precursors containing a large number of mesopores and macropores, the atomic and molecular structures of the micropores formed by the fiber are very easy to rearrange at a temperature above 1600°C. For example, the specific surface area of the boron nitride continuous fiber obtained at a temperature above 1600°C is relatively low, and the specific surface area test range is between 1-20m 2 / g, showing low porosity characteristics. In addition, a certain amount of BN bond structure has been formed inside the highly cross-linked fiber, so that the three-dimensional network of BN components inside the fiber is continuously densified, resulting in the tensile strength of the obtained boron nitride continuous fiber reaching 800 MPa (see Appendix Fig.13 As shown in Figure 2, the tensile strength reaches 800 MPa without breaking, indicating that the tensile strength can at least reach 800 MPa), while maintaining the intact fiber morphology and structure (see Appendix Figure 8-10 , Attachment Fig.15 and Figure 17-19morphology and structure characterization data).
[0096] The diameter distribution of the boron nitride continuous fibers obtained by the different filamentation methods used in the present invention is slightly different:
[0097] Among them, the diameter distribution range of the boron nitride continuous fibers obtained by electrospinning is from tens of nanometers to several microns;
[0098] Among them, the diameter distribution range of the boron nitride continuous fibers obtained by centrifugal spinning is from several hundred nanometers to several microns;
[0099] Among them, the diameter distribution range of the boron nitride continuous fiber obtained by disk spinning is from hundreds of nanometers to tens of microns;
[0100] Among them, the direct distribution range of the boron nitride continuous fibers obtained by mechanical drawing is from several microns to tens of microns.
[0101] The continuous fiber precursor provided by the present invention can be transformed into a boron nitride continuous fiber at high temperature without the participation of ammonia, and a boron nitride continuous fiber with wide diameter distribution, low porosity, high density and high mechanical strength can be obtained directly in a nitrogen environment at 1500-1800°C.
[0102] The present invention will be further described below in conjunction with the embodiments.
[0103] Example 1
[0104] (1) 210 g of cyanoguanidine and 120 g of boric acid were dissolved in 150 ml of a uniformly stirred formaldehyde aqueous solution (40 wt.%) at a constant temperature of 84° C., and the reaction was continued for 8 hours to obtain a low-crosslinked liquid resin;
[0105] (2) spinning the low-crosslinked liquid resin into continuous fibers on a disk spinning device with a rotating disk speed of 6000 r / min and an air flow temperature of 80° C. to form continuous fibers of the low-crosslinked quasi-solid resin;
[0106] (3) placing the low-crosslinked quasi-solid continuous fiber in an oven with air as hot air drying airflow, heating it to 120° C. at a heating rate of 3° C. / min, keeping it in the hot air flow at 120° C. for 30 hours, and then cooling it to room temperature at the same cooling rate to obtain a precursor of a solid resin continuous fiber with a high degree of crosslinking;
[0107] (4) The solid resin continuous fiber precursor is placed in a high-temperature heating furnace with a high-purity nitrogen protective atmosphere at a flow rate of 10-100 mL / min, and the temperature is raised to 1500-1600°C at a heating rate of 5°C / min. After reaching the target temperature, it is kept warm for 4 hours and then cooled to room temperature at the same cooling rate of 5°C / min. After the high-temperature pyrolysis reaction process, the light white fluffy substance taken out from the furnace is the boron nitride continuous fiber product.
[0108] The experimental steps mainly include low cross-linked liquid resin, low cross-linked quasi-solid resin continuous fiber, high cross-linked solid resin continuous fiber and high temperature pyrolysis reaction process to obtain boron nitride continuous fiber product (see attached for specific process) Figure 1 The boron nitride precursor fibers obtained by spinning are continuous, uniform, and fluffy, similar to the macroscopic appearance of "cotton candy" (see Appendix). Figure 2 ), based on this form, a boron nitride felt product can be prepared in one step; after compacting and high-temperature treatment, a porous block foam material constructed of boron nitride continuous fibers can be obtained (attached Figure 3 ), the block foam material has higher elasticity and higher mechanical properties.
[0109] The precursor of the highly cross-linked solid resin continuous fiber obtained in step (3) has an XRD diffraction pattern (see Figure 4 ) shows the characteristics of an ultra-wide shoulder bun diffraction peak located at about 22-25°, which shows that the resin fiber in a highly cross-linked state is a typical amorphous polymer material with a very uniform distribution of components, which is consistent with the characteristics of a highly cross-linked solid resin-type polymer.
[0110] XRD diffraction patterns of continuous fibers of highly cross-linked solid resin obtained under different pyrolysis conditions (see Appendix Figure 5 and attached Figure 6 ), wherein the high temperature treatment in nitrogen at 1500°C (as shown in the attached Figure 5 ) were observed in the diffraction pattern of (0002) and The broad shoulder diffraction peak of the crystal plane is a typical feature of the diffraction peak of the staggered hexagonal boron nitride material, indicating that the pyrolysis process in the temperature range of 1500°C forms a low crystalline phase of hexagonal boron nitride.
[0111] As a comparative example, the highly cross-linked solid resin continuous fiber was pre-treated in ammonia at 1100°C, and then the precursor fiber was pre-treated by the efficient carbon removal effect of ammonia. The fiber treated with ammonia at 1100°C was further treated at a high temperature in nitrogen at 1600°C, as a comparison with the sample in which the highly cross-linked solid resin continuous fiber was directly treated in nitrogen at 1600°C (please see the attached figure for the comparative effect). Figure 6The results show that, whether it is the direct pyrolysis treatment in a nitrogen environment at 1600°C or the high-temperature treatment process in a nitrogen environment at 1600°C after pretreatment in an ammonia environment at 1100°C, a continuous boron nitride fiber product with high crystallinity characteristics of hexagonal boron nitride can be obtained (see attached Figure 6 The XRD spectrum characteristics of the present invention are shown in Figure 2). This shows that the present invention can obtain the same pyrolysis product effect and properties as those using ammonia without using ammonia, highlighting the advantage of the present invention of using nitrogen atmosphere for direct pyrolysis.
[0112] Infrared spectra of precursor fibers (attached Figure 7 )782cm -1 The typical BN vibration peak appeared at , which confirmed the fact that a certain amount of BN bonds were formed inside the highly cross-linked resin continuous fibers, which was beneficial to keep the morphological framework formed by BN from being destroyed in the subsequent high-temperature pyrolysis treatment. Therefore, the final boron nitride phase maintained a good continuous fiber morphology (see Appendix Figure 8 , 9 and 10). Infrared spectrum (attached Figure 7 ) at 1300-1400cm -1 and 770-810cm -1 Two typical infrared vibration lines of hexagonal boron nitride appeared in the range. Figure 6 ) and SEM (attached Figure 8 , 9 The test results show that a high-purity hexagonal boron nitride continuous fiber product is obtained, with a wavelength of 3000-3800 cm -1 The vibration of -OH and -NH2 groups appeared in the range, which is a common feature of the surface of hexagonal boron nitride materials and has no direct correlation with the morphology.
[0113] Scanning electron microscopy (SEM) of boron nitride continuous fiber products Figure 8 ) analysis found that boron nitride continuous fibers are continuous and uniform, and the fiber surface is smooth and rounded when observed under a 500x magnification electron microscope.
[0114] As a comparison, Fig. 9 Figure a in the middle shows the morphology of the boron nitride continuous fiber product obtained by pre-treating the precursor fiber with ammonia at 1100℃ and then with high-purity nitrogen at 1600℃. It can be clearly seen that the surface of the fiber obtained after the ammonia pre-treatment at 1600℃ shows roughening and oriented growth of the high crystalline components of boron nitride, which will affect the mechanical properties of the fiber. In contrast, Fig. 9 Figures b and c show the morphology of the boron nitride continuous fiber product obtained by the precursor fiber after nitrogen (air content less than 1%) at 1600℃, and the attached Fig. 9Figure d in the middle shows the morphology of the boron nitride continuous fiber product obtained by pyrolysis of the precursor fiber directly in a high-purity nitrogen atmosphere at 1600°C. It can be concluded that the boron nitride fiber obtained by pyrolysis in nitrogen has obvious advantages in maintaining a better fiber structure. At the same time, it also shows that the morphology of the boron nitride continuous fiber will be significantly different due to the pyrolysis process in different atmospheres and temperatures.
[0115] Attached Fig.10 Figures c and d are the scanning morphologies of the fracture surface of Example 1. The fracture surface morphology generally presents an elliptical shape. Fig.10 Figure a is a scanned fracture of the paralleled fibers in the boron nitride continuous fiber obtained by pyrolysis with ammonia at 1100°C, and Figure b is a scanned fracture of a small amount of paralleled fibers in the fiber obtained by pyrolysis with ammonia at 1600°C. This phenomenon mainly occurs because during the transition from low cross-linking to high cross-linking, the hot air flow fails to timely separate the water byproducts generated in the high cross-linking reaction from the fiber surface, resulting in the compatible melting of the contact surface. Fig.10 Figure c in the middle is a SEM image of the fracture cross section of the boron nitride continuous fiber obtained directly at 1500℃. Fig.10 The fracture cross section of the boron nitride continuous fiber shown in Figure d becomes very smooth and flat after pyrolysis. The fracture of Figure c shows river grain characteristics, indicating that the fiber has relatively high rigidity and brittle fracture characteristics. Fig.10 Figures c and d in the figure show the representative fiber morphology and fracture characteristics of boron nitride continuous fibers obtained directly after high-temperature pyrolysis treatment at 1500℃ and 1600℃.
[0116] Nitrogen adsorption-desorption of boron nitride continuous fiber products at 77K (attached Fig.11 ) The curve test showed that the specific surface area of the boron nitride continuous fiber obtained within the temperature range of 1500℃ was 718m 2 / g, the pore distribution characteristics show the properties of being mainly concentrated in super small pores less than 4nm and micropores less than 2nm accounting for the main pore characteristics.
[0117] Attached Fig.12 The five-point BET specific surface area test dot-line graph of the fiber obtained by nitrogen pyrolysis at 1600°C in Example 1 and the comparative sample pretreated with ammonia. As can be seen from the figure, although the specific surface area of the sample in the comparative example is also relatively low, the specific surface area of the sample in Example 1 is even lower, and its specific surface area is 17.151 m 2 / g. Combined with the adsorption-desorption curve, which belongs to the typical micropore adsorption-desorption characteristics and the pore structure distribution dominated by micropores, it is shown that at high temperatures above 1600℃, the atoms or molecules in the micropores are easier to rearrange and move, causing the pore structure to collapse and disappear, achieving rapid and dense filling of the micropores (see Appendix Fig.12). Because the size of the micropores is relatively small, the volume change after rearrangement is not obvious, so this rearrangement process usually does not significantly change the overall morphology of the material. Therefore, for the boron nitride continuous fibers rich in micropores pyrolyzed at no more than 1600°C, the morphology of the material changes little after the temperature is continuously increased, but the atomic rearrangement and pore structure collapse lead to a more obvious increase in high crystallinity and high densification inside the fiber, making the overall crystallinity and mechanical properties of the fiber higher.
[0118] like Fig.13 As shown, by ion thinning the fibers obtained by pyrolysis at 1600°C and testing their tensile fracture, it was found that (see Fig.13 Figure a and Figure b, where Figure a is a real-time in-situ TEM photo before the tensile test, and Figure b is a real-time in-situ TEM photo of the fiber ion thinning area after the tensile test). The real-time monitoring in-situ image and real-time test data show that the 0.8 square micron cross section is still not broken after 638.82 micronewtons (see Fig.13 Figure c shows the relationship between the real-time load force and tensile stress of the TEM test system. It can be estimated that the mechanical tensile strength can reach a value of about 800 MPa without breaking. This test result shows that the continuous fiber obtained by the present invention has very good mechanical properties, and at the same time confirms the correctness of the densification process in which the pore structure / pores disappear by promoting the rearrangement of atoms and molecules in the microporous structure through high-temperature treatment.
[0119] On this basis, the spinning disk speed is within the range of 2000-10000r / min, the spinning air flow temperature is adjusted within the range of 50-100°C, and the heat treatment temperature of the low-crosslinked quasi-solid fiber to be converted into a highly crosslinked solid fiber can be controlled within the range of 100-350°C and the treatment time is between 24-96 hours, and the heating and cooling rates are between 1-5°C / min, to obtain a similar boron nitride continuous fiber product.
[0120] Example 2
[0121] The filamentation process in step (2) of Example 1 was changed to an electrostatic spinning process, the spinning voltage was set to 15 kV, the blowing temperature of the fan during the spinning process was 60°C, and the filaments were collected by using foil to obtain continuous fibers of low-crosslinked quasi-solid resin; the heating and cooling rates of the heat treatment in step (3) of Example 1 were adjusted to 5°C / min, the temperature was raised to 80°C and kept for 90 hours, and high-crosslinked solid resin continuous fibers were obtained; the remaining steps were the same as in Example 1. A similar boron nitride continuous fiber product can be obtained, but the overall average fiber diameter is reduced.
[0122] The continuous fiber precursor of the highly cross-linked resin obtained by spinning has continuous, oriented arrangement and a certain good mechanical strength (attached Fig.14), the boron nitride continuous fiber obtained after high temperature treatment still maintains these characteristics. Fig.15 This is a photo of the SEM scanning image of the boron nitride continuous fiber product obtained by directly placing the highly cross-linked solid resin continuous fiber in a nitrogen environment at a temperature of 1600°C. It can be observed from the figure that the diameter distribution of the boron nitride continuous fiber can extend from the quasi-nano level to the micron level, with the typical characteristics of a wide distribution. The spinning fiber can be oriented by adjusting the rotation speed of the collection hub of the spinning equipment, such as Fig.17 As shown (combined with the attached Fig.14 The actual object photo) is a photo of the SEM scanning image of the boron nitride continuous fiber film with oriented arrangement obtained in this way.
[0123] Example 2 The boron nitride continuous fiber obtained by pyrolysis at 1600°C in direct nitrogen not only has a lower porosity (see Appendix Fig.16 ), and the surface is smooth and the composition is uniform. Fine structural analysis shows that the distribution of these highly crystalline lattice staggered phases in the fiber is relatively uniform (see Fig.18 In contrast, the fibers that were previously treated with ammonia at 1100°C and then further treated at 1600°C grew densely connected, highly crystalline particles inside the fibers (see Figure 2b). Fig.18 These highly crystalline particles present a lamellar structure, but they grow together, resulting in a relatively low porosity of the fiber (see Figure 2a). Fig.16 ). With such characteristics, it can be concluded that directly using nitrogen can keep the fiber morphology structure more perfect and the porosity lower, which reflects the obvious advantage of using nitrogen for direct high-temperature pyrolysis.
[0124] On this basis, the temperature of the spinning fan is adjusted within the range of 25-70°C, and the heat treatment temperature for converting the low-crosslinked quasi-solid fiber into the highly crosslinked solid fiber can be controlled within the range of 70-350°C and the treatment time is between 24-96 hours, and the heating and cooling rates are between 1-5°C / min, and the obtained boron nitride continuous fiber product has similar properties and characteristics to those in Example 1. However, the overall fiber diameter distribution is smaller than that in Example 1.
[0125] Example 3
[0126] The low-crosslinked liquid resin in step (2) of Example 1 is mechanically drawn at room temperature to obtain a relatively thick continuous fiber of a low-crosslinked quasi-solid resin; the target temperature of the heat treatment in step (3) of Example 2 is set to 50° C. and kept warm for 90-96 hours to obtain a high-crosslinked solid resin continuous fiber; the remaining steps are the same as in Example 1. A similar boron nitride continuous fiber product can be obtained, but the total average diameter of the fiber is larger than that of Example 1.
[0127] The length of mechanically drawn continuous fibers can easily reach tens of centimeters (see Fig.19 ), under the condition of controlling the equipment well, the continuous fiber process which is the same as the above two filament forming technologies is realized. After the same high-temperature pyrolysis process as in Example 1 and Example 2, the fiber morphology remains unchanged, but the diameter of the obtained fiber can reach up to the millimeter level.
[0128] On this basis, due to the large diameter of the mechanically drawn fibers, it is necessary to adjust the heat treatment temperature of the low-crosslinked quasi-solid fiber to a high-crosslinked solid fiber and control it within the range of 35-350°C. The heating rate in the 35-100°C heating stage is very slow. Since the crude fiber of this low-crosslinked resin itself has a lot of moisture, too fast heat treatment will cause damage to the fiber structure. At the same time, it is much more difficult for the moisture by-product generated by the high crosslinking reaction to escape from the crude fiber than in Examples 1 and 2. After the temperature is higher than 100°C, the heating rate is adjusted to a maximum of 1°C / min, and the treatment time is between 50-96 hours. After the same pyrolysis process, a coarser boron nitride continuous fiber product is obtained.
[0129] Example 4
[0130] The low-crosslinked liquid resin in step (2) of Example 1 was centrifugally spun in a relatively high temperature environment, the centrifugal speed was set to 8000 r / min, and the cavity blast temperature during the spinning process was 180° C., to obtain low-crosslinked quasi-solid resin continuous fibers; the heat treatment temperature in step (3) of Example 1 was raised to 200° C. and kept warm for 2 hours to obtain highly crosslinked solid resin continuous fibers; the remaining steps were the same as in Example 1. A similar boron nitride continuous fiber product was obtained, but the average length of the total fiber was reduced.
[0131] On this basis, the centrifugal spinning speed is adjusted between 1000-8000r / min. Since the centrifugal spinning cavity is in a relatively high temperature range of 100-200°C, the moisture content of the formed low-crosslinked fiber itself is relatively low. Since the filamentation temperature is higher than that of Examples 1-3, the obtained low-crosslinked fiber itself has partially undergone high crosslinking reaction. It can be directly heat treated for a relatively short time (24-50 hours) at a relatively high heating rate of 5°C / min in a higher temperature range of 200-350°C to obtain similar boron nitride continuous fibers.
[0132] Example 5
[0133] The amount of cyanoguanidine in step (1) of Examples 1, 2, 3 and 4 is adjusted to 163 g, 180 g and 235 g, respectively, while the rest remains unchanged; or the concentration of the aqueous solution of formaldehyde in step (1) is changed to 40 wt.%, 37 wt.%, 25 wt.% and 10 wt.% respectively (or changed to an aqueous solution of acetaldehyde of the same concentration); or the volume of the formaldehyde solution is changed to 180 mL, 210 mL or 250 mL, respectively, while the rest remains unchanged, and the corresponding products have properties and characteristics similar to those of the products of Examples 1, 2, 3 and 4.
[0134] However, when the amount of solute in the solution is at its maximum, the reaction time should be extended to 48-72 hours, and the reaction temperature should be raised to the range of 80-84°C as much as possible. Too high a temperature will lead to the production of higher crosslinks, which will easily induce curing in step (1). Similarly, when the solute concentration is low, the reaction temperature can be appropriately lowered (to a temperature range of 25-80°C) or the reaction time can be shortened (to be completed within 48 hours). On this basis, other conditions remain unchanged, and a boron nitride continuous fiber product similar to that in Example 1 can be obtained.
[0135] Example 6
[0136] In step (1) of Examples 1, 2, 3, 4 and 5, an auxiliary nitrogen source is added, and the amount of the auxiliary nitrogen source added is 1%, 5% and 10% of the amount of cyanoguanidine used, and the auxiliary nitrogen source is aminoguanidine, guanidine carbonate or chlorfenapyr. After adding aminoguanidine and guanidine carbonate, it is necessary to reduce the polymerization and crosslinking of aldehyde groups and guanidine compounds, and at least one of methylamine solution (30-40wt.%), ethylene glycolamine, monoethanolamine, N-methylethanolamine, and hexamethylenetetramine is used to inhibit the crosslinking reaction; when chlorfenapyr is used, at least one of hydrochloric acid (10wt.%-37wt.%), formic acid or acetic acid is used to inhibit the crosslinking reaction; the proportion of the crosslinking inhibitor in the aqueous solution is between 6wt.% and 30wt.%; the obtained product has similar characteristics to the products of Examples 1, 2, 3, 4 and 5.
[0137] Example 7
[0138] The boric acid containing boron oxide in step (1) of Example 1 is replaced with one of boron trioxide, boric acid or borax or any combination of them. It is worth noting that when adding boron trioxide and borax, the amount of water used to convert them into boric acid should be supplemented, including boric acid and any combination of these. Other operations are the same as in Example 1, and the product obtained is similar to the boron nitride continuous fiber product of Example 1.
[0139] Example 8
[0140] The highly cross-linked resin continuous fibers in Examples 1, 2, 3, 4, 5, 6 and 7 are directly subjected to pyrolysis reaction in a nitrogen environment at a higher temperature of 1700°C or 1800°C, or the boron nitride continuous fiber products obtained in Examples 1, 2, 3, 4, 5, 6 and 7 are further heat-treated in a nitrogen environment at a higher temperature of 1700°C or 1800°C. The heating rate can be increased to 10-100°C / min, and the air flow rate can be increased to 100-1000mL / min. Other operations are the same as in Example 1. The boron nitride continuous fibers still maintain the fiber morphology unchanged, but the overall crystallinity of the fibers is further improved.
[0141] The boron nitride continuous fiber obtained by pyrolysis at a temperature range below 1500°C is replaced with ammonia or an atmosphere containing ammonia in nitrogen (ammonia volume content is within 10%), and then heat-treated at a temperature range above 1600°C. This pyrolysis process that requires low-temperature pretreatment can obtain a fiber structure with a rough fiber surface and severe grain growth inside. The fiber structure is not as perfect as the fiber structure obtained by direct pyrolysis in nitrogen (see Fig. 9 As shown in Figure a and Fig.18 ), but in general the crystallinity has similar characteristics (see Figure 6 ), and similar low surface area characteristics (see Fig.12 and Fig.16 ).
[0142] Without departing from the basic principles, basic raw materials and basic routes of the present invention, any non-inventive technology and process that replaces, simplifies, replaces, modifies, improves, modifies and adds experimental steps and raw materials to synthesize boron nitride continuous fiber products similar to those produced by the present invention, as well as any act of applying the boron nitride continuous fiber products prepared by the technology of the present invention to any field, shall be deemed as an infringement of the protection scope of the present invention.
[0143] Any matters not described in the present invention are applicable to the prior art.
Claims
1. A method for preparing boron nitride continuous fibers by filamenting aldehyde-cyanoguanidine-boryl resin, It is characterized in that The following steps are involved: (1) Low cross-linked liquid resin: A solution of an aldehyde-containing organic compound, cyanoguanidine and a boron-oxygen-containing compound are mixed and reacted under heating or room temperature to obtain a low cross-linked liquid resin that can remain in a spinnable liquid state without solidifying after being sealed and left to stand at a temperature not higher than 100° C. for at least two days; Wherein, the ratio of the mass of cyanoguanidine to the mass of the boron-oxygen compound is 1.36 to 1.95; (2) Low-crosslinked quasi-solid resin continuous fiber: The liquid resin is subjected to a filament forming process at a temperature of less than 200° C. to obtain a low-crosslinked quasi-solid resin continuous fiber; (3) Highly cross-linked solid resin continuous fibers: low-cross-linked quasi-solid resin continuous fibers are subjected to a long-term heat treatment transformation at a target temperature in the temperature range of 70-350°C to obtain dry, fully cross-linked, highly cross-linked solid resin continuous fibers, during which no bubbling occurs; (4) High-temperature pyrolysis reaction process: The highly cross-linked solid resin continuous fiber is directly subjected to high-temperature pyrolysis under a protective atmosphere to obtain a boron nitride continuous fiber.
2. The method according to claim 1, It is characterized in that In the step (1), the liquid resin with a low degree of cross-linking can still maintain a viscosity range of 10 mPa·S-10000 mPa·S after being sealed and stored for a long time for 2-100 days in a temperature range of 25° C.-84° C.
3. The method according to claim 1, It is characterized in that In the step (1), at least one auxiliary nitrogen source selected from aminoguanidine, chlorfenapyr or guanidine carbonate is added to cyanoguanidine, and the amount of the auxiliary nitrogen source added is 0wt.%-10wt.% of the mass of cyanoguanidine. At this time, a cross-linking inhibitor is added to the solution containing the aldehyde-based organic matter, and the cross-linking inhibitor is 6%-30% of the mass of the solvent in the solution; The solution containing aldehyde-based organic matter is a solution formed by dissolving formaldehyde or acetaldehyde in a solvent; wherein the solvent is a pure water solvent or a mixed solvent formed by water and a cross-linking inhibitor; and the content of formaldehyde or acetaldehyde in the solution containing aldehyde-based organic matter ranges from 10wt.% to 40wt.%.
4. The method according to claim 3, It is characterized in that The cross-linking inhibitor is at least one of methylamine solution (30-40 wt.%), ethylene glycolamine, monoethanolamine, N-methylethanolamine, hexamethylenetetramine, hydrochloric acid (10 wt.%-37 wt.%), formic acid or acetic acid.
5. The method according to claim 1, It is characterized in that The ratio of the mass of the cyanoguanidine (in grams) to the volume of the solution containing the aldehyde organic matter (in milliliters) is 0.7 to 1.6; The boron-oxygen compound is at least one of boron trioxide, boric acid or borax.
6. The method according to claim 1, It is characterized in that In the step (2), the filament forming process is to form the liquid resin into a continuous fiber of a low-crosslinked quasi-solid resin by a filament forming technology including electrospinning, centrifugal spinning, disc spinning or mechanical drawing; Among them, the voltage of electrospinning is 10-30 kV, and the fan blowing temperature ranges from 25-70°C during the spinning process; The centrifugal spinning speed is 1000-8000r / min, and the blast temperature in the centrifugal spinning collection chamber is in the range of 100-200°C; The rotating disk speed of the disc spinning is 2000-10000r / min, and the temperature range of the blowing air flow provided in the disc spinning collection space is 50-100℃; Among them, the temperature range of mechanical wire drawing is 25-35℃.
7. The method according to claim 1, It is characterized in that In the step (3), the heating rate during the process of converting the low-crosslinked quasi-solid resin fiber into the highly crosslinked solid resin fiber after a long period of heat treatment under normal pressure air environment is not higher than 5°C / min, and the low-crosslinked quasi-solid resin fiber is exposed in a heating-drying device purged with a hot air flow, and the fiber formed after the high crosslinking conversion is completed does not contain any water molecule components, and any water molecule components include bound water, free water and water products; In the step (4), the heating / cooling rate during high-temperature pyrolysis is 5-100°C / min, the protective atmosphere is high-purity nitrogen or nitrogen, ammonia, or a mixture of ammonia and nitrogen with a volume content of less than or equal to 1% in air, and the gas flow rate is 10-1000ml / min; The high temperature pyrolysis temperature is 1500-1800°C, the pyrolysis time is 0.5-24 hours, and the pyrolysis atmosphere is nitrogen, high-purity nitrogen, or ammonia-nitrogen mixed gas with an ammonia volume content of less than 10%; Alternatively, the high-temperature pyrolysis is carried out in two stages, the first stage pyrolysis temperature is 1100-1400°C, the protective atmosphere is ammonia or a mixture of ammonia and nitrogen, the second stage pyrolysis temperature is 1600-1800°C, the protective atmosphere is nitrogen, and the total pyrolysis time is 0.5-24 hours.
8. A boron nitride continuous fiber obtained by the method according to any one of claims 1 to 7, It is characterized in that The diameter distribution of BN continuous fibers extends from nanometer to micrometer.
9. The boron nitride continuous fiber according to claim 8, It is characterized in that When the high temperature pyrolysis target temperature is not less than 1600℃, the specific surface area of the boron nitride continuous fiber is between 1-20m 2 / g range, the tensile strength of the boron nitride continuous fiber is not less than 800MPa.
10. A product using the boron nitride continuous fiber according to claim 8 or 9, It is characterized in that The boron nitride continuous fibers are made into boron nitride fiber felt, boron nitride fiber film, boron nitride fiber paper, boron nitride fiber cloth, boron nitride fiber block foam, and boron nitride fiber-reinforced ceramic-based, polymer-based or metal-based composite materials.
Citation Information
Cited By
Bacteriostatic deodorizing fabric and preparation process thereof
CN119332364A
Bacteriostatic and deodorant fabric and preparation process thereof
CN119332364B