Waveguide sheet soft film imprinting method and waveguide sheet
Through the soft film embossing method of waveguide sheets with thick coatings and glue layers on the carrier film and wafer surfaces, the surface defect problem in nanoimprinting technology is solved, and the product appearance quality and yield are improved.
Patent Information
- Application Number
- CN202411119993.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The existing nanoimprinting technology can easily lead to scratches, foreign objects and concave and bumps on the wafer surface during the transfer process, resulting in poor product appearance quality and affecting performance.
By using the waveguide sheet soft film embossing method, a coating and glue layer of more than 3 μm is formed on the carrier film and wafer surface, the grating pattern is transferred to the wafer with pressure applied, and the curing process is performed to peel off the carrier film, fill and cover. Surface defects.
It significantly improves the appearance quality of the product, reduces the scrap rate caused by surface defects, and improves the appearance yield from 50% to 90%.
Smart Images

Figure CN118915384A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of transfer technology, and in particular to a waveguide soft film stamping method and a waveguide. Background Art
[0002] The current nanoimprint technology can easily cause defects such as scratches, foreign matter, and bumps on the wafer surface during the transfer process, resulting in poor appearance quality of the transferred product and affecting product performance. Summary of the invention
[0003] In view of this, the present application proposes a waveguide soft film imprinting method and a waveguide, which can effectively fill and cover the defects on the surface of the carrier film and the surface of the wafer during the transfer process, greatly improving the appearance quality of the product, reducing the scrap rate caused by surface defects, and improving the appearance yield.
[0004] The first aspect of the present application provides a waveguide soft film imprinting method, comprising:
[0005] Providing a carrier film and a wafer, wherein the carrier film has a grating pattern;
[0006] Processing a coating with a thickness of more than 3 μm on a surface of the carrier film facing the wafer;
[0007] Processing the surface of the wafer facing the carrier film to form a glue layer with a thickness of more than 3 μm;
[0008] Attaching the carrier film to the wafer so that the coating on the surface of the carrier film contacts the adhesive layer on the surface of the wafer;
[0009] Applying pressure to transfer the grating pattern on the carrier film to the wafer;
[0010] The wafer is cured, and the carrier film is peeled off from the wafer to leave the wafer containing the grating pattern, thereby completing the transfer.
[0011] In some embodiments, the step of forming a coating having a thickness of 3 μm or greater on the surface of the carrier film facing the wafer comprises:
[0012] A micro-concave coating process or a slit coating process is adopted to form a uniform coating with a thickness of 3 μm-5 μm on the surface of the carrier film.
[0013] In some embodiments, the step of forming a glue layer with a thickness of 3 μm or greater on the surface of the wafer facing the carrier film comprises:
[0014] A spin coating process is used to coat the surface of the wafer to form a uniform adhesive layer with a thickness of 3 μm-5 μm.
[0015] In some embodiments, the spin coating process is used to coat the wafer surface with a glue layer having a thickness of 3 μm-5 μm, including:
[0016] providing a liquid coating material;
[0017] Dropping the liquid coating material on the surface of the wafer so that the liquid coating material can evenly cover the entire surface of the wafer;
[0018] The rotation speed is controlled to be 1000 rpm-2000 rpm, and the wafer is driven to rotate so as to form a uniform adhesive layer with a thickness of 3 μm-5 μm on the surface of the wafer.
[0019] In some embodiments, applying pressure to transfer the grating pattern on the carrier film to the wafer includes:
[0020] placing the carrier film and the wafer on an imprinting device;
[0021] Set the imprinting parameters;
[0022] After the carrier film is aligned with the wafer, the imprinting device is started to transfer the grating pattern on the carrier film to the wafer.
[0023] In some embodiments, setting the imprint parameters comprises:
[0024] Adjust the imprint pressure to within 5000Pa, set the imprint speed to 1mm / s-2mm / s, and adjust the imprint angle to 5°-10°.
[0025] In some embodiments, the carrier film is a polycarbonate film.
[0026] In some embodiments, the coating is at least one of acrylate, vinyl, and polyurethane.
[0027] In some embodiments, the step of peeling the carrier film from the wafer includes:
[0028] Adjust the demoulding angle to 5°-10° to match the embossing angle.
[0029] A second aspect of the present application provides a waveguide plate manufactured by the above-mentioned imprinting method.
[0030] The waveguide soft film imprinting method and waveguide proposed in the present application can effectively fill and cover the defects on the surface of the carrier film and the surface of the wafer by accurately controlling the thickness of the coating and the adhesive layer. This greatly improves the appearance quality of the product, reduces the scrap rate caused by surface defects, and improves the appearance yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained like these drawings without paying any creative work.
[0032] Figure 1 This is a schematic diagram of the structure of the carrier film coating proposed in this application;
[0033] Figure 2 This is a schematic diagram of the structure of the wafer coating adhesive layer proposed in this application;
[0034] Figure 3 This is a schematic diagram of the process of the imprinting method proposed in this application.
[0035] Description of reference numerals:
[0036] 10. Carrier film; 11. Coating layer; 20. Adhesive layer; 30. Wafer. DETAILED DESCRIPTION
[0037] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0038] It should be understood that all directional indications in the embodiments of the present application (such as up, down, left, right, front, back, etc.) are only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.
[0039] It should also be understood that when an element is referred to as being "fixed" or "disposed on" another element, it can be directly on the other element or there may be an intermediate element at the same time. When an element is referred to as being "connected" to another element, it can be directly connected to the other element or it can be indirectly connected to the other element through an intermediate element.
[0040] The terms used in this specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. For example, the descriptions of "first", "second", etc. in the present application are only for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features.
[0041] It should be further understood that the term “and / or” used in the specification and appended claims refers to any combination and all possible combinations of one or more of the associated listed items, and includes these combinations.
[0042] The current nanoimprint technology can easily cause defects such as scratches, foreign matter, and bumps on the wafer surface during the transfer process, resulting in poor appearance quality of the transferred product and affecting product performance.
[0043] For example, in the field of AR diffraction optical waveguides, when preparing diffraction waveguides, it is necessary to set a diffraction grating pattern on a carrier film and apply a coating on the carrier film. The coating thickness commonly used in the industry is generally 0.2μm-0.3μm. It is also necessary to apply a glue layer on the surface of the wafer. The glue layer thickness commonly used in the industry is generally 1μm-2μm. The diffraction grating pattern on the carrier film is transferred to the wafer surface through an imprinting device.
[0044] However, the configuration of the above coating is prone to cause defects such as scratches, foreign matter and bumps on the surface during the transfer process, and due to the thin thickness of the adhesive layer, it cannot effectively fill and cover the surface defects, resulting in poor appearance quality of the product after transfer, affecting product performance and high scrap rate.
[0045] Specifically, surface defects mainly include bumps and concave spots, foreign matter (dust particles, etc.), dirt (oil stains, etc.) on the carrier film and wafer. These defects are inherent in the carrier film raw materials and introduced during the wafer surface processing (dust particles, oil stains, etc.).
[0046] Therefore, the embodiment of the present application proposes a waveguide soft film imprinting method and a waveguide, which can effectively fill and cover the defects on the surface of the carrier film and the surface of the wafer during the transfer process, greatly improving the appearance quality of the product, reducing the scrap rate caused by surface defects, and improving the appearance yield.
[0047] See also Figures 1 to 3 The present application provides a waveguide soft film imprinting method, comprising:
[0048] S1, providing a carrier film 10 and a wafer 30, wherein the carrier film 10 has a grating pattern;
[0049] S2, forming a coating 11 with a thickness of more than 3 μm on the surface of the carrier film 10 facing the wafer 30;
[0050] S3, forming a glue layer 20 with a thickness of more than 3 μm on the surface of the wafer 30 facing the carrier film 10;
[0051] S4, attaching the carrier film 10 to the wafer 30, so that the coating 11 on the surface of the carrier film 10 is in contact with the adhesive layer 20 on the surface of the wafer 30;
[0052] S5, applying pressure to transfer the grating pattern on the carrier film 10 to the wafer 30;
[0053] S6, performing a curing process on the wafer 30, peeling the carrier film 10 from the wafer 30, so as to leave the wafer 30 containing the grating pattern, and completing the transfer.
[0054] The imprinting method of the embodiment of the present application fills and reduces surface defects in a covering manner by using the coating 11 on the thickened carrier film 10 and the adhesive layer 20 on the wafer 30, so that the two opposite surfaces of the carrier film 10 and the wafer 30 can obtain a flat plane, so no defect marks will be generated due to particles or oil during imprinting, and at the same time, by setting the thickness of the coating coated on the surface of the wafer 30 to be above 3μm, it can not only eliminate the influence of dust and oil, but also ensure the imprinting effect, and will not cause the optical performance of the waveguide after imprinting, such as light efficiency, uniformity, MTF, etc., to deteriorate due to excessive thickness, thereby ensuring the optical performance of the product, greatly improving the appearance quality of the product, reducing the scrap rate caused by surface defects, and improving the appearance yield. After quality appearance inspection, the appearance performance is improved from the original 50% yield to 90% yield.
[0055] In some embodiments, the imprinting method of the present application can be applied to the field of AR diffraction optical waveguides, and the carrier film 10 can be a polymer film such as a polycarbonate film (PC film), and the adhesive layer 20 is a photoresist.
[0056] In some embodiments, the coating 11 may be made of at least one of acrylate, vinyl ester, and polyurethane. The above materials have good adhesion, wear resistance, and high temperature resistance to ensure that the grating pattern can be transferred to the wafer 30 with high quality.
[0057] In some embodiments, in step S2, a coating layer 11 of more than 3 μm is formed on the surface of the carrier film 10 facing the wafer 30, including: using a micro-concave coating process or a slit coating process to form a uniform coating layer 11 with a thickness of 3 μm-5 μm on the surface of the carrier film 10. During the processing, it is relatively difficult to ensure the thickness and uniformity of the coating layer 11. Therefore, the embodiment of the present application can meet the requirements of high-precision coating through the micro-concave coating process or the slit coating process to form a coating layer 11 with uniform thickness.
[0058] Exemplarily, the micro-concave coating process uses a gravure roller with a smaller diameter, and does not use the traditional lamination back roller coating method, but uses two closely spaced matching rollers with the same (or close) roller diameters to fully flatten the carrier film 10 and make slight contact with the gravure roller. The coating after scraping and metering by the scraper is evenly spread on the surface of the gravure roller, and continuously contacts the carrier film 10 with the rotation of the gravure roller to form a wetting line. The relative movement of the carrier film 10 and the gravure roller completes the uniform transfer of the coating from the gravure roller to the carrier film 10, thereby forming a coating 11 with uniform thickness.
[0059] Illustratively, slit coating technology is a high-precision coating method that uses an extremely fine nozzle and a high-precision coating system to squeeze and spray viscous liquid or paste materials along the gap of the coating mold at a certain pressure and a certain flow rate and transfer them to the carrier film 10, thereby forming a coating 11 with uniform thickness.
[0060] Exemplarily, the thickness of the coating 11 can be 3 μm, 4 μm or 5 μm, etc. Setting the thickness of the coating 11 within the above range can effectively fill and cover the defects on the surface of the carrier film 10, greatly improve the appearance quality of the product, reduce the scrap rate caused by surface defects, and reduce production costs.
[0061] In some embodiments, in step S3, the surface of the wafer 30 facing the carrier film 10 is processed to form a glue layer 20 of more than 3 μm, including: using a spin coating process to form a uniform glue layer 20 with a thickness of 3 μm-5 μm on the surface of the wafer 30. During the processing, it is relatively difficult to ensure the thickness and uniformity of the glue layer 20. Therefore, the embodiment of the present application can achieve high-precision preparation of the glue layer 20 through the spin coating process, so that the thickness and uniformity of the glue layer 20 can be effectively controlled.
[0062] For example, the spin coating process relies on the centrifugal force and gravity generated when the wafer 30 rotates to spread the liquid coating material (such as photoresist) on the surface of the wafer 30 to form a uniform adhesive layer 20. By controlling parameters such as the rotation speed, the thickness and uniformity of the adhesive layer 20 can be precisely controlled.
[0063] Exemplarily, the thickness of the adhesive layer 20 can be 3μm, 4μm or 5μm, etc. Setting the thickness of the adhesive layer 20 within the above range can effectively fill and cover the defects on the surface of the wafer 30, greatly improve the appearance quality of the product, reduce the scrap rate caused by surface defects, and reduce production costs.
[0064] The imprinting method of the embodiment of the present application optimizes the thickness of the coating 11 coated on the surface of the carrier film 10 and the adhesive layer 20 coated on the surface of the wafer 30, and selects a specific process (micro-concave coating process or slit coating process and spin coating process) so that the two opposite surfaces of the carrier film 10 and the wafer 30 can obtain a flat plane, so no defect marks will be generated due to particles and oil during imprinting. At the same time, by setting the thickness of the coating coated on the surface of the wafer 30 to 3-5 microns, the influence of dust and oil can be eliminated and the imprinting effect can be guaranteed. The optical performance of the waveguide after imprinting, such as light efficiency, uniformity, MTF, etc., will not deteriorate due to excessive thickness.
[0065] In some embodiments, in step S3, a uniform adhesive layer 20 with a thickness of 3 μm-5 μm is formed on the surface of the wafer 30 by a spin coating process, including:
[0066] S31, providing a liquid coating material, such as a photoresist, etc.
[0067] S32, dripping the liquid coating material onto the surface of the wafer 30, so that the liquid coating material can evenly cover the entire surface of the wafer 30;
[0068] S33, controlling the rotation speed to be 1000 rpm-2000 rpm, and driving the wafer 30 to rotate by the rotating device to form a uniform adhesive layer with a thickness of 3 μm-5 μm on the surface of the wafer 30.
[0069] During the spin coating process, the rotation speed has a significant effect on the thickness of the adhesive layer 20. Generally, the higher the rotation speed, the greater the centrifugal force, and the thinner the thickness of the adhesive layer 20. Too low a rotation speed may cause the thickness of the adhesive layer 20 to be uneven and cause edge effects; while too high a rotation speed may cause the adhesive layer 20 to be too thin or even crack. The embodiment of the present application limits the rotation speed to a range of 1000 rpm to 2000 rpm. Within this range, the thickness and uniformity of the adhesive layer 20 can be accurately controlled to obtain an adhesive layer 20 of better quality.
[0070] Therefore, by controlling the rotation speed within the range of 1000rpm-2000rpm, the surface of the wafer 30 can be coated with a glue layer 20 with a thickness of 3μm-5μm, thereby effectively filling and covering the defects on the surface of the wafer 30, greatly improving the appearance quality of the product, reducing the scrap rate caused by surface defects, and reducing production costs.
[0071] For example, the rotation speed may be controlled to be 1000 rpm, 1100 rpm, 1200 rpm, 1300 rpm, 1400 rpm, 1500 rpm, 1600 rpm, 1700 rpm, 1800 rpm, 1900 rpm or 2000 rpm, etc. The thickness of the adhesive layer 20 may be precisely controlled within the range of 3 μm-5 μm by adjusting the rotation speed.
[0072] In some embodiments, in step S5, applying pressure to transfer the grating pattern on the carrier film 10 to the wafer 30 includes:
[0073] S41, placing the carrier film 10 and the wafer 30 on an imprinting device;
[0074] S42, setting imprinting parameters, such as imprinting pressure, imprinting speed, and imprinting angle.
[0075] S43 , after aligning the carrier film 10 with the wafer 30 , start the imprinting equipment to transfer the grating pattern on the carrier film 10 to the wafer 30 .
[0076] In some embodiments, in step S42, setting the imprint parameters includes: adjusting the imprint pressure to within 5000Pa, setting the imprint speed to 1mm / s-2mm / s, and adjusting the imprint angle to 5°-10°. Thus, the imprint pressure is adjusted to within 5000Pa to ensure that the grating pattern can be completely and clearly transferred to the wafer while avoiding damage to the wafer. The imprint speed is set to 1mm / s-2mm / s to ensure that the pattern can be evenly and stably transferred to the wafer during the imprint process. The imprint angle is adjusted to 5°-10° to ensure the uniformity and accuracy of the grating pattern transfer. By adjusting the above parameters, the performance of the imprinted product is up to standard and stable.
[0077] Exemplarily, the embossing angle can be adjusted to 5°, 6°, 7°, 8°, 9° or 10°. By setting the above-mentioned embossing angle, the fluidity of the material can be improved, so that the material can more evenly fill the nanostructure in the mold, that is, the adhesive layer 20 can flow smoothly and evenly fill the nanostructure formed by the grating pattern of the carrier film 10, thereby helping to reduce the formation of bubbles and other defects to ensure the accurate replication of the grating pattern.
[0078] In addition, since the material may be subjected to uneven stress distribution during the stamping process, resulting in stress concentration, and then cracks or other forms of material failure, the above risks can be effectively reduced by adjusting the stamping angle to 5°-10°.
[0079] In some embodiments, in step S6 , the wafer 30 is cured by heating, ultraviolet irradiation, etc., to enhance the bonding force between the grating pattern and the wafer.
[0080] In some embodiments, in step S6, the step of peeling the carrier film 10 from the wafer 30 includes: adjusting the demolding angle to 5°-10° to match the imprinting angle to reduce deformation or damage of the pattern during the demolding process. Exemplarily, the demolding angle can be adjusted to 5°, 6°, 7°, 8°, 9° or 10°.
[0081] In practical applications, the embossing process and the demoulding process are completed on the same platform. The embossing operation is performed first, then UV ultraviolet light exposure and curing is performed, and finally demoulding is performed. The entire process does not require the platform to be changed. The embossing process and the demoulding process can maintain an upward or downward angle of 5°-10° relative to the horizontal plane. Any angle can be selected within the range of 5°-10° for demoulding according to specific needs.
[0082] The demoulding angle matches the embossing angle, which means that the demoulding angle and the embossing angle are both maintained within the range of 5°-10°. The specific values of the demoulding angle and the embossing angle may be the same or different, as long as they are maintained within the range of 5°-10°.
[0083] The embodiment of the present application also provides a waveguide sheet, which is manufactured by the above-mentioned embossing method. Therefore, the above-mentioned embossing method improves the appearance quality of the manufactured waveguide sheet, reduces the scrap rate caused by surface defects, and improves the appearance yield.
[0084] Those skilled in the art may combine and associate different embodiments or examples and features of different embodiments or examples described in this specification without mutual contradiction.
[0085] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed in the present application, and these modifications or replacements should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.
Claims
1. A waveguide soft film imprinting method, It is characterized in that include: Providing a carrier film and a wafer, wherein the carrier film has a grating pattern; Processing a coating with a thickness of more than 3 μm on a surface of the carrier film facing the wafer; Processing the surface of the wafer facing the carrier film to form a glue layer with a thickness of more than 3 μm; Attaching the carrier film to the wafer so that the coating on the surface of the carrier film contacts the adhesive layer on the surface of the wafer; Applying pressure to transfer the grating pattern on the carrier film to the wafer; The wafer is cured, and the carrier film is peeled off from the wafer to leave the wafer containing the grating pattern, thereby completing the transfer.
2. The imprinting method according to claim 1, It is characterized in that The processing of forming a coating with a thickness of more than 3 μm on the surface of the carrier film facing the wafer comprises: A micro-concave coating process or a slit coating process is adopted to form a uniform coating with a thickness of 3 μm-5 μm on the surface of the carrier film.
3. The imprinting method according to claim 2, It is characterized in that The step of processing the surface of the wafer facing the carrier film to form a glue layer with a thickness of more than 3 μm comprises: A spin coating process is used to coat the surface of the wafer to form a uniform adhesive layer with a thickness of 3 μm-5 μm.
4. The imprinting method according to claim 3, It is characterized in that The method of using a spin coating process to coat the wafer surface with a glue layer having a thickness of 3 μm-5 μm includes: providing a liquid coating material; Dropping the liquid coating material on the surface of the wafer so that the liquid coating material can evenly cover the entire surface of the wafer; The rotation speed is controlled to be 1000 rpm-2000 rpm, and the wafer is driven to rotate so as to form a uniform adhesive layer with a thickness of 3 μm-5 μm on the surface of the wafer.
5. The imprinting method according to claim 4, It is characterized in that The applying pressure to transfer the grating pattern on the carrier film to the wafer includes: placing the carrier film and the wafer on an imprinting device; Set the imprint parameters; After the carrier film is aligned with the wafer, the imprinting device is started to transfer the grating pattern on the carrier film to the wafer.
6. The imprinting method according to claim 5, It is characterized in that The setting of the imprinting parameters comprises: Adjust the imprint pressure to within 5000Pa, set the imprint speed to 1mm / s-2mm / s, and adjust the imprint angle to 5°-10°.
7. The embossing method according to any one of claims 1 to 6, It is characterized in that The carrier film is a polycarbonate film.
8. The embossing method according to any one of claims 1 to 6, It is characterized in that The coating is at least one of acrylate, vinyl ester and polyurethane.
9. The imprinting method according to claim 6, It is characterized in that The step of peeling the carrier film from the wafer comprises: Adjust the demoulding angle to 5°-10° to match the embossing angle.
10. A waveguide sheet, It is characterized in that The invention is prepared by the embossing method as described in any one of claims 1 to 9.
Citation Information
Patent Citations
Surface protection film fabrication method and fabrication apparatus and surface protection film
CN103958157A
Preparation method of transfer ink
CN111703230A
Nanoimprint soft film and preparation method thereof
CN115356797A
Micro-Conformal Templates for Nanoimprint Lithography
US20110183027A1