Surface anti-corrosion treatment method for stator shell of marine generator
Through the Ni-TiPorous Sintered Coating and Hot Dip Galvanized Combination Treatment, the corrosion problem of marine generator stator shell in harsh environments is solved, and significant corrosion resistance and service life are achieved.
Patent Information
- Application Number
- CN202411009996.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The stator shell of marine generators is prone to corrosion in harsh environments, and the prior art is difficult to effectively prevent corrosion, resulting in insufficient service performance and life.
The porous sintered coating is made by mixing nickel powder and titanium powder, and the pores are filled with hot dip galvanizing treatment to form a composite anticorrosion coating. Combined with high-temperature sintering and low-melting zinc liquid, the corrosion resistance of the coating is enhanced.
It significantly improves the corrosion resistance and corrosion resistance of the stator shell, extends the service life of marine generators and their stator shells, and avoids coating peeling and anti-corrosion failure.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of corrosion protection of marine generator equipment, and in particular relates to a surface corrosion protection treatment method for a stator shell of a marine generator. Background Art
[0002] Marine generators include marine diesel generators, marine gas turbine generators, etc. The working environment of marine generators is obviously harsh, including: high oil, high temperature, high humidity, high pollution, high salt air and high salt seawater in the marine environment, etc. Since the stator shell of the marine generator is usually made of steel materials, and since the stator shell is usually directly exposed to the air and directly in contact with the outside oil, sewage, dirt, marine air, seawater, etc., the stator shell of the marine generator must be treated with anti-corrosion to ensure the normal use, performance and service life of the marine generator and its stator shell.
[0003] Therefore, how to optimize the surface anti-corrosion treatment of the stator casing of the marine generator, improve the corrosion resistance of the stator casing, and thereby improve the performance and service life of the marine generator and its stator casing is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention
[0004] The purpose of the present invention is to provide a surface anti-corrosion treatment method for a stator shell of a marine generator.
[0005] In order to achieve the above object, the technical solution of the present invention is as follows:
[0006] A surface anticorrosion treatment method for a stator housing of a marine generator comprises the following steps performed in sequence:
[0007] 1) mixing nickel powder and titanium powder evenly, then ball milling, then adding water and a binder while mixing and evenly mixing to form a slurry, then brushing the slurry evenly on the exposed surface of the stator shell, then drying, then placing in a vacuum drying oven for vacuum drying, then vacuum sintering, argon atmosphere sintering or nitrogen atmosphere sintering, then cooling with the furnace, after cooling is completed, taking out of the furnace, and sintering a porous sintered nickel-titanium coating on the surface of the stator shell;
[0008] 2) Hot-dip galvanizing: The stator shell with the porous sintered nickel-titanium coating on the surface obtained in step 1) is pickled, washed with water, and dipped in a plating agent in sequence, and then the stator shell is immersed in the zinc liquid in the zinc pot in the hot-dip galvanizing furnace for hot-dip galvanizing treatment. After immersion for a period of time, the stator shell is taken out of the zinc liquid, and then the zinc liquid on the stator shell is cooled and solidified. After solidification, a composite anti-corrosion coating formed by the porous sintered nickel-titanium coating and the hot-dip galvanized layer is obtained on the surface of the stator shell.
[0009] Preferably, in step 1), the purity of the nickel powder and the titanium powder by mass percentage is 99.9%-99.99%;
[0010] The particle size of nickel powder and titanium powder is 20 microns to 200 microns;
[0011] The mass of nickel powder: the mass of titanium powder = 1:(2-3).
[0012] Preferably, in step 1), the binder is polyvinyl alcohol, and the mass percentage of polyvinyl alcohol in the slurry is 0.2%-1%;
[0013] The exposed surfaces of the stator housing that are painted include the inner and outer surfaces of the wall panels of the box-shaped stator housing.
[0014] Preferably, in step 1), the insulation temperature of the vacuum drying treatment is 70°C-90°C.
[0015] Preferably, in step 1), the holding temperature of vacuum sintering, argon atmosphere sintering or nitrogen atmosphere sintering is 1200° C.-1400° C., and the holding time is 5 h-15 h.
[0016] Preferably, in step 2), the temperature of the zinc liquid in the zinc pot is 435° C.-460° C., and the thickness of the hot-dip galvanized layer is 35 μm-100 μm.
[0017] The present application has achieved the following beneficial technical effects:
[0018] In the present application, a porous sintered nickel-titanium coating is prepared by a slurry sintering method, which makes full use of the excellent corrosion resistance of nickel and titanium, so that the porous sintered nickel-titanium coating has excellent and relatively high corrosion resistance and anti-corrosion effect, and the porous sintered nickel-titanium coating improves the corrosion resistance and anti-corrosion effect of the surface of the stator housing;
[0019] Furthermore, since the nickel powder particles and titanium powder particles are both spherical in shape with an outer diameter of 20-200 microns, and sintering is not melting, sintering only realizes point contact and point connection between adjacent particles, the sintered coating is a porous coating with a large number of pores between adjacent particles. The non-complete melting characteristics of sintering at a sintering temperature below the melting point determine that the pores between the adjacent particles are inevitable, must exist, and exist in large quantities, and the pores can always reach the original surface of the stator housing matrix after going around, thus causing the outside world to Oil, sewage, dirt, ocean air, seawater, etc. will gradually penetrate inward along the pores until they reach the original surface of the stator housing substrate, thereby weakening the anti-corrosion effect of the sintered nickel-titanium coating; for this reason, the present application subsequently adds another hot-dip galvanizing treatment, using a low-melting-point, highly fluid zinc liquid to infiltrate and fill the above-mentioned pores, and the zinc liquid in the pores will be cooled and solidified to fill and seal the pores. In this way, the porous sintered nickel-titanium coating uses hot-dip galvanizing to achieve pore filling and sealing, thereby improving the corrosion resistance and anti-corrosion effect of the porous sintered nickel-titanium coating;
[0020] In the present application, the hot-dip galvanized layer itself has relatively high corrosion resistance and anti-corrosion effect, and the hot-dip galvanized layer improves the corrosion resistance and anti-corrosion effect of the surface of the stator housing;
[0021] However, if hot-dip galvanizing is performed directly, the temperature of the zinc liquid during hot-dip galvanizing is only about 440°C, which is low, resulting in the inherently weak bonding strength between the hot-dip galvanized layer and the surface of the stator housing. This is determined and limited by the principle of hot-dip galvanizing, which causes the hot-dip galvanized layer to easily peel off after a long period of use, thereby causing anti-corrosion failure. For this reason, the present application first sintered a layer of porous structure coating on the surface of the stator housing. Since the porous sintered coating is sintered at a high temperature of 1200°C-1400°C, which is much higher than the 440°C of hot-dip galvanizing, the porous sintered coating and its The bonding strength between the particles in the porous sintered coating and the surface of the stator housing is much higher than that of hot-dip galvanizing. Since there are a large number of pores in the porous sintered coating, these pores are formed into anchor piles firmly fixed on the surface of the stator housing, so that the hot-dip galvanized zinc liquid can be hidden in the pores, and the zinc liquid is wrapped, anchored and pulled by the firmly fixed and strong pores. Due to the anchoring and pulling effect of the pores, the peeling problem of the hot-dip galvanized layer caused by external forces is reduced, thereby improving the corrosion resistance and anti-corrosion effect of the hot-dip galvanized layer.
[0022] In summary, since both the porous sintered nickel-titanium coating and the hot-dip galvanized layer have relatively high corrosion resistance and anti-corrosion effect, and further since the porous sintered nickel-titanium coating and the hot-dip galvanized layer help each other, borrow from each other, complement each other, and combine to improve the corrosion resistance and anti-corrosion effect of the surface of the composite anti-corrosion coating and the stator casing, thereby improving the performance and service life of the marine generator and its stator casing. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. The described embodiments are only part of the embodiments of the present invention, not all of them. Therefore, based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] The present application provides a surface anti-corrosion treatment method for a stator housing of a marine generator, comprising the following steps performed in sequence:
[0025] 1) mixing nickel powder and titanium powder evenly, then ball milling, then adding water and a binder while mixing and evenly mixing to form a slurry, then brushing the slurry evenly on the exposed surface of the stator shell, then drying, then placing in a vacuum drying oven for vacuum drying, then vacuum sintering, argon atmosphere sintering or nitrogen atmosphere sintering, then cooling with the furnace, after cooling is completed, taking out of the furnace, and sintering a porous sintered nickel-titanium coating on the surface of the stator shell;
[0026] 2) Hot-dip galvanizing: The stator shell with the porous sintered nickel-titanium coating on the surface obtained in step 1) is pickled, washed with water, and dipped in a plating agent in sequence, and then the stator shell is immersed in the zinc liquid in the zinc pot in the hot-dip galvanizing furnace for hot-dip galvanizing treatment. After immersion for a period of time, the stator shell is taken out of the zinc liquid, and then the zinc liquid on the stator shell is cooled and solidified. After solidification, a composite anti-corrosion coating formed by the porous sintered nickel-titanium coating and the hot-dip galvanized layer is obtained on the surface of the stator shell.
[0027] In one embodiment of the present application, in step 1), the purity of the nickel powder and the titanium powder by mass percentage is 99.9%-99.99%;
[0028] The particle size of nickel powder and titanium powder is 20 microns to 200 microns;
[0029] The mass of nickel powder: the mass of titanium powder = 1:(2-3).
[0030] In one embodiment of the present application, in step 1), the binder is polyvinyl alcohol, and the mass percentage of polyvinyl alcohol in the slurry is 0.2%-1%;
[0031] The exposed surfaces of the stator housing that are painted include the inner and outer surfaces of the wall panels of the box-shaped stator housing.
[0032] In one embodiment of the present application, in step 1), the insulation temperature of the vacuum drying treatment is 70°C-90°C.
[0033] In one embodiment of the present application, in step 1), the holding temperature of vacuum sintering, argon atmosphere sintering or nitrogen atmosphere sintering is 1200° C.-1400° C., and the holding time is 5 h-15 h.
[0034] In one embodiment of the present application, in step 2), the temperature of the zinc liquid in the zinc pot is 435° C.-460° C., and the thickness of the hot-dip galvanized layer is 35 μm-100 μm.
[0035] In the present application, titanium is a hard, shiny, silvery-white metal with a melting point of 1668°C and a boiling point of 3287°C; nickel is a hard, ductile, ferromagnetic metal that is highly polishable and corrosion-resistant. For example, a large amount of nickel is added to stainless steel, and the melting point of nickel is 1453°C; the melting point of zinc is 419.53°C, and the boiling point of zinc is 907°C.
[0036] In the present application, hot-dip galvanizing is the process of placing a metal workpiece into molten metal to form a coating on its surface, such as hot-dip galvanizing, hot-dip aluminum, etc. The most widely used steel materials in industry will corrode to varying degrees when used in environments such as the atmosphere, seawater, soil, and building materials. Hot-dip galvanizing is one of the effective means to delay environmental corrosion of steel materials. It is to immerse the steel products whose surfaces have been cleaned and activated in molten zinc liquid, and to coat the surface of the steel products with a zinc coating through the reaction and diffusion between iron and zinc. The hot-dip galvanizing process has obvious advantages in the protective characteristics of the combination of the physical barrier and electrochemical protection of the coating, the density, maintenance-freeness and economy of the coating, and its adaptability to the shape and size of the product.
[0037] The methods and devices not described in detail in the present invention are all prior art and will not be described in detail.
[0038] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.
[0039] Example 1
[0040] A surface anticorrosion treatment method for a stator housing of a marine generator comprises the following steps performed in sequence:
[0041] 1) mixing nickel powder and titanium powder evenly, then ball milling, then adding water and a binder while mixing and evenly mixing to form a slurry, then brushing the slurry evenly on the exposed surface of the stator shell, then drying, then placing in a vacuum drying oven for vacuum drying, then vacuum sintering, then cooling with the furnace, taking out of the furnace after cooling is completed, and sintering a porous sintered nickel-titanium coating on the surface of the stator shell;
[0042] In step 1), the purity of the nickel powder and the titanium powder by mass percentage is 99.9%-99.99%;
[0043] The particle size of nickel powder and titanium powder is 50 microns to 100 microns;
[0044] The mass of nickel powder: the mass of titanium powder = 1:3;
[0045] In step 1), the binder is polyvinyl alcohol, and the mass percentage of polyvinyl alcohol in the slurry is 0.25%;
[0046] Painting the exposed surface of the stator housing by brushing includes the inner surface and the outer surface of the wall plate of the stator housing;
[0047] In step 1), the holding temperature of the vacuum drying treatment is 80°C;
[0048] In step 1), the vacuum sintering temperature is 1400° C. and the holding time is 12 h;
[0049] 2) Hot-dip galvanizing: the stator shell with the porous sintered nickel-titanium coating on the surface obtained in step 1) is pickled, washed with water, and dipped in a plating agent in sequence, and then the stator shell is immersed in the zinc liquid in the zinc pot in the hot-dip galvanizing furnace for hot-dip galvanizing treatment, and after immersion for a period of time, the stator shell is fished out from the zinc liquid, and then the zinc liquid on the stator shell is cooled and solidified, and after solidification, a composite anti-corrosion coating formed by the porous sintered nickel-titanium coating and the hot-dip galvanized layer is obtained on the surface of the stator shell;
[0050] In step 2), the temperature of the zinc liquid in the zinc pot is 445° C.-455° C., and the thickness of the hot-dip galvanized layer is 35 μm-50 μm.
[0051] Example 2
[0052] A surface anticorrosion treatment method for a stator housing of a marine generator comprises the following steps performed in sequence:
[0053] 1) mixing nickel powder and titanium powder evenly, then ball milling, then adding water and a binder while mixing and evenly mixing to form a slurry, then brushing the slurry evenly on the exposed surface of the stator shell, then drying, then placing in a vacuum drying oven for vacuum drying, then sintering in an argon atmosphere, then cooling with the furnace, taking out of the furnace after cooling is completed, and sintering a porous sintered nickel-titanium coating on the surface of the stator shell;
[0054] In step 1), the purity of the nickel powder and the titanium powder by mass percentage is 99.9%-99.99%;
[0055] The particle size of nickel powder and titanium powder is 40 microns to 80 microns;
[0056] The mass of nickel powder: the mass of titanium powder = 1:3;
[0057] In step 1), the binder is polyvinyl alcohol, and the mass percentage of polyvinyl alcohol in the slurry is 0.3%;
[0058] Painting the exposed surface of the stator housing by brushing includes the inner surface and the outer surface of the wall plate of the stator housing;
[0059] In step 1), the holding temperature of the vacuum drying treatment is 75°C;
[0060] In step 1), the holding temperature of argon atmosphere sintering is 1390° C. and the holding time is 14 h;
[0061] 2) Hot-dip galvanizing: the stator shell with the porous sintered nickel-titanium coating on the surface obtained in step 1) is pickled, washed with water, and dipped in a plating agent in sequence, and then the stator shell is immersed in the zinc liquid in the zinc pot in the hot-dip galvanizing furnace for hot-dip galvanizing treatment, and after immersion for a period of time, the stator shell is fished out from the zinc liquid, and then the zinc liquid on the stator shell is cooled and solidified, and after solidification, a composite anti-corrosion coating formed by the porous sintered nickel-titanium coating and the hot-dip galvanized layer is obtained on the surface of the stator shell;
[0062] In step 2), the temperature of the zinc liquid in the zinc pot is 440° C.-450° C., and the thickness of the hot-dip galvanized layer is 35 μm-40 μm.
[0063] Example 3
[0064] A surface anticorrosion treatment method for a stator housing of a marine generator comprises the following steps performed in sequence:
[0065] 1) mixing nickel powder and titanium powder evenly, then ball milling, then adding water and a binder while mixing and evenly mixing to form a slurry, then brushing the slurry evenly on the exposed surface of the stator shell, then drying, then placing in a vacuum drying oven for vacuum drying, then sintering in a nitrogen atmosphere, then cooling with the furnace, taking out of the furnace after cooling is completed, and sintering a porous sintered nickel-titanium coating on the surface of the stator shell;
[0066] In step 1), the purity of the nickel powder and the titanium powder by mass percentage is 99.9%-99.99%;
[0067] The particle size of nickel powder and titanium powder is 50 microns to 70 microns;
[0068] The mass of nickel powder: the mass of titanium powder = 1:3;
[0069] In step 1), the binder is polyvinyl alcohol, and the mass percentage of polyvinyl alcohol in the slurry is 0.2%;
[0070] Painting the exposed surface of the stator housing by brushing includes the inner surface and the outer surface of the wall plate of the stator housing;
[0071] In step 1), the holding temperature of the vacuum drying treatment is 80°C;
[0072] In step 1), the holding temperature of the sintering in nitrogen atmosphere is 1380°C-1390°C, and the holding time is 13h;
[0073] 2) Hot-dip galvanizing: the stator shell with the porous sintered nickel-titanium coating on the surface obtained in step 1) is pickled, washed with water, and dipped in a plating agent in sequence, and then the stator shell is immersed in the zinc liquid in the zinc pot in the hot-dip galvanizing furnace for hot-dip galvanizing treatment, and after immersion for a period of time, the stator shell is fished out from the zinc liquid, and then the zinc liquid on the stator shell is cooled and solidified, and after solidification, a composite anti-corrosion coating formed by the porous sintered nickel-titanium coating and the hot-dip galvanized layer is obtained on the surface of the stator shell;
[0074] In step 2), the temperature of the zinc liquid in the zinc pot is 435° C.-445° C., and the thickness of the hot-dip galvanized layer is 35 μm-43 μm.
[0075] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A surface anti-corrosion treatment method for a stator housing of a marine generator, characterized in that: The method includes the following steps: 1) mixing nickel powder and titanium powder evenly, then ball milling, then adding water and a binder while mixing and evenly mixing to form a slurry, then brushing the slurry evenly on the exposed surface of the stator shell, then drying, then placing in a vacuum drying oven for vacuum drying, then vacuum sintering, argon atmosphere sintering or nitrogen atmosphere sintering, then cooling with the furnace, after cooling is completed, taking out of the furnace, and sintering a porous sintered nickel-titanium coating on the surface of the stator shell; 2) Hot-dip galvanizing: The stator shell with the porous sintered nickel-titanium coating on the surface obtained in step 1) is pickled, washed with water, and dipped in a plating agent in sequence, and then the stator shell is immersed in the zinc liquid in the zinc pot in the hot-dip galvanizing furnace for hot-dip galvanizing treatment. After immersion for a period of time, the stator shell is taken out of the zinc liquid, and then the zinc liquid on the stator shell is cooled and solidified. After solidification, a composite anti-corrosion coating formed by the porous sintered nickel-titanium coating and the hot-dip galvanized layer is obtained on the surface of the stator shell.
2. The surface anticorrosion treatment method of the stator housing of a marine generator according to claim 1, characterized in that: In step 1), the purity of the nickel powder and the titanium powder by mass percentage is 99.9%-99.99%; The particle size of nickel powder and titanium powder is 20 microns to 200 microns; The mass of nickel powder: the mass of titanium powder = 1:(2-3).
3. The surface anti-corrosion treatment method of the stator housing of a marine generator according to claim 1, characterized in that: In step 1), the binder is polyvinyl alcohol, and the mass percentage of polyvinyl alcohol in the slurry is 0.2%-1%; The exposed surfaces of the stator housing that are painted include the inner and outer surfaces of the wall panels of the box-shaped stator housing.
4. The surface anticorrosion treatment method of the stator housing of a marine generator according to claim 1, characterized in that: In step 1), the insulation temperature of the vacuum drying treatment is 70°C-90°C.
5. The surface anti-corrosion treatment method of the stator housing of a marine generator according to claim 1, characterized in that: In step 1), the holding temperature of vacuum sintering, argon atmosphere sintering or nitrogen atmosphere sintering is 1200° C.-1400° C., and the holding time is 5 h-15 h.
6. The surface anticorrosion treatment method of the stator housing of a marine generator according to claim 1, characterized in that: In step 2), the temperature of the zinc liquid in the zinc pot is 435° C.-460° C., and the thickness of the hot-dip galvanized layer is 35 μm-100 μm.