Anti-aging antirust heat shrink film and preparation method thereof

Through the design of aging-resistant and anti-rust-resistant heat shrink film with a three-layer structure, the traditional heat shrink film is solved in rust-resistant and anti-ultraviolet-resistant masterbatches, combined with metallocene polyethylene and linear low-density polyethylene materials. The shortcomings in aging have achieved durable and comprehensive protection of metal components.

CN118927747APending Publication Date: 2024-11-12VCI ANTIRUST NEW MATERIALS SHANGHAI
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411012775.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional heat shrink films cannot effectively prevent metal parts from rusting and aging and decomposing in harsh environments, limiting their application for long-term outdoor use.

Method used

Aging-resistant and anti-rust-resistant heat shrink film design with a three-layer structure, in which the inner layer film contains gas-phase anti-rust masterbatches to prevent rust, the middle layer and outer layer film contain UV-resistant aging masterbatches, combining metallocene polyethylene and linear low density Polyethylene materials are prepared by extrusion blow molding process to ensure the stability and protective effect of the film under harsh conditions.

Benefits of technology

It significantly extends the anti-rust period of metal parts, enhances the weather resistance and physical properties of the membrane material, and provides comprehensive protection, including dustproof, moisture-proof, and damage-proof, and is suitable for wind power, automobiles and boilers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004964867110000071
    Figure BDA0004964867110000071
Patent Text Reader

Abstract

The invention relates to the field of heat shrinkage films, and particularly discloses an anti-aging and anti-rust heat shrinkage film and a preparation method thereof. The anti-aging and anti-rust heat shrinkage film sequentially comprises an inner layer film, a middle layer film and an outer layer film from inside to outside, the inner layer film comprises metallocene polyethylene, LDPE and gas-phase anti-rust master batches, the middle layer film comprises metallocene polyethylene, LDPE and anti-ultraviolet and anti-aging master batches, and the outer layer film comprises, by weight, metallocene polyethylene, LDPE and anti-ultraviolet and anti-aging master batches; the preparation method comprises the following steps: carrying out extrusion blow molding at 190-220 DEG C to obtain an inner layer film; carrying out extrusion blow molding at 200-230 DEG C to obtain a middle layer film; carrying out extrusion blow molding at 240-260 DEG C to obtain an outer layer film; and stacking the three prepared films according to the sequence of inner layer-middle layer-outer layer, extruding, and cooling and shaping by a cooling roller to obtain the anti-aging and anti-rust thermal shrinkage film. The anti-aging and anti-rust heat shrinkage film has the advantages of being resistant to corrosion, high in weather resistance and resistant to aging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of heat shrinkable films, and more specifically, to an aging-resistant and rust-proof heat shrinkable film and a preparation method thereof. Background Art

[0002] In the rapidly developing packaging industry, heat shrink film technology is gradually becoming an indispensable part of many industries as an efficient, environmentally friendly and multifunctional packaging solution. The characteristic of heat shrink film is that it can shrink significantly in size after being heated, tightly fit and wrap the packaged items, forming an almost seamless protective layer, effectively protecting the product from the external environment, while improving the overall aesthetics and market competitiveness of the product.

[0003] The origin of heat shrink film technology can be traced back to the middle of the last century. With the continuous progress of polymer material science and the increasing maturity of plastic processing technology, heat shrink film has gradually moved from the laboratory to industrial production. In the early days, this technology was mainly used in the field of food packaging, especially the fresh-keeping packaging of perishable foods such as meat, fruits and vegetables. With the continuous innovation of technology and the expansion of market demand, the application scope of heat shrink film has rapidly expanded to electronic products, auto parts, daily chemical products, stationery and even medicine, becoming an indispensable part of the modern packaging industry.

[0004] With the continuous expansion of the application field of heat shrink film, its application demand in large-scale wind power, automobiles, boilers and other fields is also increasing. However, traditional heat shrink film materials are mainly made of polymer materials such as polyolefins. Its main function is to provide physical protection, such as dustproof, moisture-proof, and anti-breakage, but it cannot effectively prevent the rust of metal parts. On the other hand, due to the complex and changeable outdoor environment, such as high temperature and ultraviolet rays can cause the film material to soften and deform and accelerate the aging and decomposition of the film material, making the metal equipment covered by the film material susceptible to the influence of environmental temperature and humidity and corrosive substances in the atmosphere, making the metal parts easy to rust and damage, thereby limiting its long-term use outdoors. Summary of the invention

[0005] In order to solve the above problems, the present application provides an aging-resistant and rust-proof heat shrinkable film and a preparation method thereof.

[0006] In the first aspect, the present application provides an aging-resistant and rust-proof heat shrinkable film, which adopts the following technical solution: An aging-resistant and rust-proof heat shrinkable film comprises, from the inside to the outside, an inner layer film, a middle layer film and an outer layer film, wherein the inner layer film components comprise, by weight, 10-30 parts of metallocene polyethylene, 30-60 parts of LDPE, and 5-10 parts of vapor phase antirust masterbatch, the middle layer film components comprise, by weight, 10-30 parts of metallocene polyethylene, 30-60 parts of LDPE, and 5-10 parts of anti-ultraviolet and aging-resistant masterbatch, and the outer layer film components comprise, by weight, 20-50 parts of metallocene polyethylene, 20-50 parts of LDPE, and 10-20 parts of anti-ultraviolet and aging-resistant masterbatch.

[0007] By adopting the above technical solution, vapor phase anti-rust masterbatch is specially added to the inner film. This masterbatch can continuously release anti-rust gas in a certain space, forming a protective film covering the surface of metal parts, effectively preventing moisture, oxygen and other corrosive substances from direct contact with metals, thereby significantly extending the anti-rust period of metal parts and protecting them from rust damage. This is particularly important for equipment that uses a large number of metal parts in industries such as wind power, automobiles, and boilers. Anti-ultraviolet and anti-aging masterbatches are added to the middle and outer films. These masterbatches can effectively absorb or reflect ultraviolet rays, reduce the direct damage of ultraviolet rays to the film material, and enhance the weather resistance of the film material to prevent softening deformation and aging decomposition caused by long-term exposure to the outdoor environment. This design ensures that the heat shrink film can maintain stable physical properties and protective effects under various harsh climatic conditions. The entire film structure is based on metallocene polyethylene and linear low-density polyethylene as the main substrates. Both materials have good mechanical strength and flexibility, so that the heat shrink film can provide anti-rust and anti-aging protection while also effectively resisting physical damage, such as dust, moisture, and damage, and fully protecting the covered object. This aging-resistant and rust-proof heat shrinkable film effectively solves the shortcomings of traditional heat shrinkable films in rust prevention and aging resistance through an innovative three-layer structure design and the addition of functional masterbatch, providing more comprehensive and lasting protection for equipment in large-scale wind power, automobiles, boilers and other fields.

[0008] Optionally, the vapor phase anti-rust masterbatch includes a combination of capric acid, caprylic acid, sebacic acid, benzoic acid, monoethanolamine and urotropine in a mass ratio of (1-1.5):(1-1.5):(0.5-1):(2.5-3.5):(1-1.5):(1.5-2).

[0009] By adopting the above technical solution, through a special ratio of capric acid, caprylic acid, sebacic acid, benzoic acid, monoethanolamine and urotropine combination, the vapor phase rust-proof masterbatch can release rust-proof gas when heated. These gases can quickly form a dense protective film on the metal surface, effectively isolating corrosive substances such as water vapor and oxygen, thereby significantly enhancing the anti-rust effect.

[0010] Optionally, the anti-ultraviolet and anti-aging masterbatch comprises, by weight, 0.1-2 parts of hindered amine light stabilizer, 1-3 parts of ultraviolet absorber, 3-5 parts of composite antioxidant, 0.1-0.5 parts of silane coupling agent, and 0.3-0.8 parts of lubricant.

[0011] Optionally, the hindered amine light stabilizer includes bis(2,2,6,6-tetramethyl-4-hydroxypiperidinyl) sebacate.

[0012] Optionally, the ultraviolet absorber includes 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole.

[0013] Optionally, the composite antioxidant includes two or three of amine antioxidants, ester antioxidants, and phenolic antioxidants.

[0014] By adopting the above technical solution, hindered amine light stabilizers, such as bis(2,2,6,6-tetramethyl-4-hydroxypiperidinyl) sebacate, can capture free radicals and prevent the photooxidation reaction, thereby effectively delaying the aging of the film due to ultraviolet radiation. In addition, hindered amine light stabilizers also have a certain self-repairing ability and can form a protective layer on the surface of the film to further resist the damage of ultraviolet rays.

[0015] UV absorbers, such as 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole, can strongly absorb ultraviolet rays and convert them into harmless heat or long-wave radiation, thereby avoiding direct damage to the membrane material by ultraviolet rays. This mechanism effectively reduces the destructive effect of ultraviolet rays on the molecular chain of the membrane material and prolongs the service life of the membrane material.

[0016] Composite antioxidants are composed of two or three of amine antioxidants, ester antioxidants, and phenol antioxidants. They each have different mechanisms of action and work together in the aging process of the membrane material. Amine antioxidants mainly capture peroxyl free radicals, ester antioxidants prevent the chain reaction by decomposing hydroperoxides, and phenol antioxidants can capture free radicals and decompose hydroperoxides at the same time. This composite action allows the antioxidant to exert a good antioxidant effect in a wider temperature range, further improving the aging resistance of the membrane material.

[0017] Silane coupling agent plays a bridging role in anti-ultraviolet and anti-aging masterbatch. It can improve the interfacial bonding between inorganic fillers and organic polymers, and improve the mechanical properties and anti-aging properties of composite materials. In film materials, silane coupling agent helps to enhance the flexibility and tear resistance of film materials, and also helps to improve the adhesion between film materials and metal parts, preventing the film materials from falling off during use.

[0018] Optionally, the lubricant includes stearamide.

[0019] In a second aspect, the present application provides a method for preparing an aging-resistant and rust-proof heat shrinkable film, which adopts the following technical solution: A method for preparing an aging-resistant and rust-proof heat shrinkable film comprises the following steps: After mixing the components of the inner layer film, the films are extruded and blow-molded at 190-220°C to obtain the inner layer film; the middle layer film components are extruded and blow-molded at 200-230°C to obtain the middle layer film; the outer layer film components are extruded and blow-molded at 240-260°C to obtain the outer layer film; the three films prepared are stacked in the order of inner layer-middle layer-outer layer, and are cooled and formed by extrusion and cooling rollers to obtain an aging-resistant and rust-proof heat shrinkable film.

[0020] By adopting the above technical solution, the extrusion blow molding process enables each layer of the film to be formed evenly and continuously, ensuring the thickness consistency and surface flatness of the film. The three films prepared are precisely stacked in the order of inner layer-middle layer-outer layer, ensuring the stability of the film structure and the full play of the anti-rust and aging resistance properties. Through extrusion and cooling and shaping with cooling rollers, the three layers of film are closely combined to form a composite film with excellent performance. In this process, the cooling effect of the cooling roller helps to quickly shape the film, so that the composite film has excellent performance in flexibility, tear resistance, weather resistance and other aspects.

[0021] In summary, this application has the following beneficial effects: 1. Since the anti-aging and anti-rust heat shrink film of this application innovatively adopts a three-layer structure design, the inner layer incorporates vapor phase anti-rust masterbatch to extend the anti-rust period of metal parts, and the middle and outer layers add anti-ultraviolet and anti-aging masterbatch, which significantly improves the weather resistance of the film material and resists the influence of ultraviolet rays and bad climate. With metallocene polyethylene and LDPE as the base material, combined with excellent mechanical strength and flexibility, it is not only anti-rust and anti-aging, but also fully protects against dust, moisture and damage, providing long-lasting and comprehensive protection for equipment in the fields of wind power, automobiles, boilers, etc.

[0022] 2. In this application, the gas phase antirust masterbatch is preferably composed of precisely proportioned capric acid, caprylic acid, sebacic acid, benzoic acid, monoethanolamine and urotropine, and its mass ratio is carefully designed to ensure that the antirust gas can be efficiently released when heated. These gases quickly form a solid protective film on the metal surface, effectively blocking corrosion factors such as moisture and oxygen, greatly improving the antirust performance, and providing excellent antirust protection for the heat shrink film.

[0023] 3. The method of this application ensures the best performance and consistency of each layer of material through the temperature-layered extrusion blow molding process. The precise stacking and cooling shaping process finally produces a three-layer composite film that exhibits excellent performance in rust prevention, aging resistance and physical properties, providing a reliable solution for metal protection. DETAILED DESCRIPTION

[0024] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.

[0025] Preparation example of vapor phase anti-rust masterbatch Preparation Example 1 Preparation of a gas phase anti-rust masterbatch: 13 kg of capric acid, 12 kg of caprylic acid, 8 kg of sebacic acid, 30 kg of benzoic acid, 12 kg of monoethanolamine and 18 kg of urotropine were mixed in a clean container, and stirred evenly by a stirrer to obtain a vapor phase antirust masterbatch.

[0026] Preparation Example 2 Preparation of a gas phase anti-rust masterbatch: 10 kg of capric acid, 10 kg of caprylic acid, 5 kg of sebacic acid, 25 kg of benzoic acid, 10 kg of monoethanolamine and 15 kg of urotropine were mixed in a clean container, and stirred evenly by a stirrer to obtain a vapor phase antirust masterbatch.

[0027] Preparation Example 3 Preparation of a gas phase anti-rust masterbatch: 15 kg of capric acid, 15 kg of caprylic acid, 10 kg of sebacic acid, 35 kg of benzoic acid, 15 kg of monoethanolamine and 20 kg of urotropine were mixed in a clean container, and stirred evenly by a stirrer to obtain a vapor phase antirust masterbatch.

[0028] Preparation example of anti-ultraviolet and anti-aging masterbatch Preparation Example 4 Preparation of UV-resistant and aging-resistant masterbatch: 10 kg of bis(2,2,6,6-tetramethyl-4-hydroxypiperidinyl) sebacate, 20 kg of 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole, 20 kg of diethyldiphenylamine, 20 kg of dilauryl thiodipropionate, 3 kg of silane coupling agent and 5 kg of stearamide were mixed evenly in a clean stirring tank, and hot-melt granulation was performed at 260±10°C to obtain an anti-UV and anti-aging masterbatch.

[0029] Preparation Example 5 Preparation of UV-resistant and aging-resistant masterbatch: The difference from Preparation Example 4 is that the composite antioxidant is 20 kg of dilauryl thiodipropionate and 20 kg of 2,6-di-tert-butyl-p-cresol.

[0030] Preparation Example 6 Preparation of UV-resistant and aging-resistant masterbatch: The difference from Preparation Example 4 is that the composite antioxidant is 20 kg of diethyldiphenylamine and 20 kg of 2,6-di-tert-butyl-p-cresol.

[0031] Preparation Example 7 Preparation of UV-resistant and aging-resistant masterbatch: The difference from Preparation Example 4 is that the composite antioxidant is 13 kg of diethyldiphenylamine, 14 kg of dilauryl thiodipropionate, and 13 kg of 2,6-di-tert-butyl-p-cresol.

[0032] Preparation Example 8 Preparation of UV-resistant and aging-resistant masterbatch: The difference from Preparation Example 4 is that the composite antioxidant is a mixture of 20 kg of antioxidant 1010 and 20 kg of antioxidant 245. Example

[0033] Example 1 Preparation method of aging-resistant and rust-proof heat shrinkable film: Prepare 20kg of metallocene polyethylene and 45kg of a density of 0.91g / cm 3 LDPE and 8kg of gas phase antirust masterbatch are used as the inner layer film preparation materials, and 20kg of metallocene polyethylene and 45kg of density 0.91g / cm 3 LDPE, 8kg anti-ultraviolet and anti-aging masterbatch as the middle layer film preparation material, prepare 35kg metallocene polyethylene, 35kg density of 0.91g / cm 3 LDPE and 15kg of anti-ultraviolet and anti-aging masterbatch are used as materials for preparing the outer layer film, wherein the vapor phase anti-rust masterbatch is prepared by Preparation Example 1, the anti-ultraviolet and anti-aging masterbatch is prepared by Preparation Example 4, and the metallocene polyethylene is purchased from ExxonMobil; Using a twin-screw extruder, the inner layer material is extruded and blown at 200°C to form a film, so as to obtain an inner layer film with a thickness of 0.08±0.03mm; the middle layer material is extruded and blown at 220°C to form a film, so as to obtain a middle layer film with a thickness of 0.08±0.03mm; the outer layer material is extruded and blown at 250°C to form an outer layer film with a thickness of 0.08±0.03mm; The three films prepared were stacked in the order of inner layer-middle layer-outer layer, extruded by a roller press at a force of 2 MPa, and then transported to a cooling roller for cooling and shaping to obtain an aging-resistant and rust-proof heat shrinkable film.

[0034] Example 2 Preparation method of aging-resistant and rust-proof heat shrinkable film: The difference from Example 1 is that the vapor phase antirust masterbatch is prepared by Preparation Example 2.

[0035] Example 3 Preparation method of aging-resistant and rust-proof heat shrinkable film: The difference from Example 1 is that the vapor phase antirust masterbatch is prepared by Preparation Example 3.

[0036] Example 4 Preparation method of aging-resistant and rust-proof heat shrinkable film: The difference from Example 1 is that the anti-ultraviolet and aging-resistant masterbatch is prepared by Preparation Example 5.

[0037] Example 5 Preparation method of aging-resistant and rust-proof heat shrinkable film: The difference from Example 1 is that the anti-ultraviolet and aging-resistant masterbatch is prepared by Preparation Example 6.

[0038] Example 6 Preparation method of aging-resistant and rust-proof heat shrinkable film: The difference from Example 1 is that the anti-ultraviolet and aging-resistant masterbatch is prepared by Preparation Example 7.

[0039] Example 7 Preparation method of aging-resistant and rust-proof heat shrinkable film: The difference from Example 1 is that the anti-ultraviolet and aging-resistant masterbatch is prepared by Preparation Example 8.

[0040] Comparative Example Comparative Example 1 The method for preparing an aging-resistant and rust-proof heat shrinkable film is different from Example 1 in that the metallocene polyethylene is replaced by polyethylene.

[0041] Comparative Example 2 Preparation method of aging-resistant and rust-proof heat shrinkable film: The difference from Example 1 is that no vapor phase antirust masterbatch is added to the inner layer film.

[0042] Comparative Example 3 Preparation method of aging-resistant and rust-proof heat shrinkable film: The difference from Example 1 is that no anti-ultraviolet and aging-resistant masterbatch is added to the middle layer film and the outer layer film.

[0043] Performance testing Detection Methods Changes in physical properties of samples before and after aging: Test thickness, tensile strength and elongation respectively. Refer to ISO 527-1-2019 method, test speed: 100mm / min, test environment: 23±2℃, 50±5%RH, pre-conditioning conditions: 23±2℃, 24 hours.

[0044] VIA Vapor Phase Corrosion Inhibition Test: The test is carried out according to the method specified in TL8135-0002.

[0045] Vapor phase rust-proof materials are divided into 4 levels: Level 3: no rust; Level 2: rust 20%; Level 1: rust 20%-80%; Level 0: The rust area is more than 80%.

[0046] Table 1 Changes in physical properties of samples before and after aging Table 2 VIA gas phase corrosion inhibition test VCI Grade Example 1 Level 3 Example 2 Level 3 Example 3 Level 3 Example 4 Level 3 Example 5 Level 3 Example 6 Level 3 Example 7 Level 3 Comparative Example 1 Level 2 Comparative Example 2 Level 1 Comparative Example 3 Level 2 Combining Example 1 and Comparative Example 1 with Tables 1-2, it can be seen that the metallocene linear low-density polyethylene significantly improves the aging resistance of the heat shrink film with its unique molecular chain structure and excellent thermal stability. In harsh environments such as high temperature and ultraviolet rays, the metallocene linear low-density polyethylene can effectively resist the breakage and degradation of the molecular chain, thereby extending the service life of the film material.

[0047] Combining Example 1 and Comparative Example 2 with Tables 1-2, it can be seen that the vapor phase anti-rust masterbatch can continuously volatilize VCI (vapor phase corrosion inhibitor) anti-rust gas. This anti-rust gas can adhere to the metal surface with a molecular thickness to form a protective film, effectively isolating the metal from moisture and oxygen in the air, thereby preventing the metal from rusting.

[0048] Combining Example 1 and Comparative Example 3 with Tables 1-2, it can be seen that the anti-ultraviolet and anti-aging masterbatch can efficiently absorb ultraviolet energy and convert it into harmless heat energy release, thereby avoiding ultraviolet rays directly damaging polymer chains, significantly delaying the aging process of the material, and reducing the photo-oxidative degradation caused by ultraviolet rays. The composite antioxidant is composed of a variety of antioxidants, which can work synergistically to provide more comprehensive and lasting antioxidant protection, not only effectively capture and remove free radicals, but also form a stable protective layer inside the material to prevent the penetration of oxygen and other oxidants, thereby extending the service life of the material.

[0049] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. An anti-aging and anti-rust heat shrinkable film, characterized in that: From the inside to the outside, it includes an inner layer film, a middle layer film and an outer layer film. The inner layer film components include 10-30 parts by weight of metallocene polyethylene, 30-60 parts by weight of LDPE, and 5-10 parts by weight of vapor phase anti-rust masterbatch; the middle layer film components include 10-30 parts by weight of metallocene polyethylene, 30-60 parts by weight of LDPE, and 5-10 parts by weight of anti-UV and anti-aging masterbatch; the outer layer film components include 20-50 parts by weight of metallocene polyethylene, 20-50 parts by weight of LDPE, and 10-20 parts by weight of anti-UV and anti-aging masterbatch.

2. The anti-aging and anti-rust heat shrinkable film according to claim 1, characterized in that: The vapor phase antirust masterbatch comprises a combination of capric acid, caprylic acid, sebacic acid, benzoic acid, monoethanolamine and urotropine in a mass ratio of (1-1.5):(1-1.5):(0.5-1):(2.5-3.5):(1-1.5):(1.5-2).

3. The anti-aging and anti-rust heat shrinkable film according to claim 1, characterized in that: The anti-ultraviolet and anti-aging masterbatch comprises, by weight, 0.1-2 parts of hindered amine light stabilizer, 1-3 parts of ultraviolet absorber, 3-5 parts of composite antioxidant, 0.1-0.5 parts of silane coupling agent and 0.3-0.8 parts of lubricant.

4. The anti-aging and anti-rust heat shrinkable film according to claim 3, characterized in that: The hindered amine light stabilizer includes bis(2,2,6,6-tetramethyl-4-hydroxypiperidinyl) sebacate.

5. The anti-aging and anti-rust heat shrinkable film according to claim 3, characterized in that: The ultraviolet absorber includes 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole.

6. The anti-aging and anti-rust heat shrinkable film according to claim 3, characterized in that: The composite antioxidant comprises two or three of amine antioxidants, ester antioxidants and phenol antioxidants.

7. The anti-aging and anti-rust heat shrinkable film according to claim 3, characterized in that: The lubricant includes stearamide.

8. A method for preparing an aging-resistant and rust-proof heat shrinkable film according to any one of claims 1 to 7, characterized in that: The following steps are involved: The inner layer film components are mixed and then extruded and blow molded at 190-220°C to obtain an inner layer film; the middle layer film components are extruded and blow molded at 200-230°C to obtain a middle layer film; and the outer layer film components are extruded and blow molded at 240-260°C to obtain an outer layer film; The three films prepared are stacked in the order of inner layer-middle layer-outer layer, and are shaped by extrusion and cooling with cooling rollers to obtain an aging-resistant and rust-proof heat shrinkable film.

Citation Information

Patent Citations

  • Nano composite modifying agent for improving weathering resistance performance powder paint and preparation method thereof

    CN101362868A

  • Flame-retardant shrinkable anticorrosive packaging film and manufacturing method thereof

    CN102029755A

  • VCI high-tensile heat-shrinkable antirust film

    CN109291577A

  • Cross-linking thermal shrinkage film with rust prevention function and preparing method thereof

    CN110408109A

  • Degradable rust-proof master batch, preparation method of degradable rust-proof master batch, degradable gas-phase rust-proof film containing degradable rust-proof master batch and application

    CN111978698A