Concrete composite additive for crack resistance and preparation method thereof
By using composite additives with specific components in concrete and preparation methods, the shortcomings of improving concrete performance in complex environments are solved, and crack resistance and strength are significantly improved. It is suitable for concrete engineering in high-altitude areas.
Patent Information
- Application Number
- CN202411065966.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The existing composite admixtures have limited effect on improving concrete performance in complex environments such as low temperature and wind, especially in crack-resistant concrete projects in high-altitude areas, and the formulation and preparation process are not clear.
A type of water including deionized water, polymer monomers, modified polycarboxylic acid water reducing agent, gas induction agent, nanosilica, ultrafine fly ash, emulsifier, tackifier, urea and hydraulic lime are used. Composite additives are prepared by a specific stirring process to form a concrete composite additive for crack resistance, reducing the water-cement ratio and introducing stable bubbles, improving the working performance and strength of concrete.
It significantly improves the crack resistance and working performance of concrete, reduces the amount of cement, reduces the cost of raw materials, and increases the strength and density of concrete, and is suitable for concrete projects in complex environments.
Smart Images

Figure CN118930114A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of concrete admixtures, and specifically relates to a concrete composite additive for crack resistance and a preparation method thereof. Background Art
[0002] Concrete admixtures refer to chemical substances added during concrete production to change certain specific properties of concrete or achieve specific functions. According to different functions, admixtures can be divided into various types such as reinforcing agents, water reducing agents, retarders, early strength agents, bubbling agents, densifiers, waterproofing agents, antifreeze agents, etc. In response to the needs of concrete construction in complex environments, composite admixtures are generally used to improve the performance of concrete.
[0003] At present, general composite admixtures such as air-entraining water-reducing agents, although they can improve the working performance of concrete, are not suitable for concrete projects in complex environments. General composite admixtures have very limited effect on improving the performance of concrete in complex and changeable environments such as low temperature and windy conditions, and the formula and preparation process of composite admixtures developed for anti-cracking concrete projects in high-cold areas are still unclear. Therefore, it is urgent to find a formula and preparation process for anti-cracking concrete admixtures that can entrain air to stabilize foam and "reduce glue and strengthen". Summary of the invention
[0004] In order to solve the above problems, the object of the present invention is to provide a concrete composite additive for crack resistance.
[0005] The present invention also aims to provide a method for preparing the above-mentioned concrete composite additive for crack resistance;
[0006] In order to achieve the above object, the technical solution of the present invention is implemented as follows: a concrete composite additive for crack resistance, the concrete composite additive specifically comprises the following components in parts by weight: deionized water: 100 parts;
[0007] Polymer monomer: 50-80 parts;
[0008] Modified polycarboxylic acid water reducer: 5-25 parts;
[0009] Air entraining agent: 10-20 parts;
[0010] Nano silicon dioxide: 5-15 parts;
[0011] Ultrafine fly ash: 10-15 parts;
[0012] Emulsifier: 5-8 parts;
[0013] Tackifier: 3-6 parts;
[0014] Urea: 2-4 parts;
[0015] Hydraulic lime: 2-4 parts;
[0016] Preferably, the polymer monomer is at least one of butyl methacrylate and hydroxyethyl methacrylate.
[0017] Preferably, the air entraining agent is sodium dodecylbenzene sulfonate.
[0018] Preferably, the viscosity increasing agent is polyacrylamide.
[0019] Another technical solution of the present invention is achieved as follows: a method for preparing a composite concrete additive for crack resistance, the method specifically comprising:
[0020] After adding the emulsifier to deionized water and heating it to 30-40°C, the polymer monomer and the viscosity enhancer are added and stirred evenly, and then heated to 55-65°C, the water reducer, air entraining agent, nano-silicon dioxide, ultrafine fly ash and hydrated lime are added and stirred evenly, and then cooled to room temperature to obtain a composite additive for crack-resistant concrete. The polymer monomer is added twice, and the initial addition amount is 20-40%.
[0021] Preferably, the stirring time after adding the polymer monomer and the tackifier is 1-2 hours.
[0022] Preferably, the stirring time after adding the water reducing agent, the air entraining agent, the nano-silicon dioxide, the ultrafine fly ash and the hydrated lime is 2.5-3.5 hours.
[0023] Compared with the prior art, by applying the concrete composite additive of the present invention to concrete, the working performance of the crack-resistant concrete can be improved by reducing the water-cement ratio and introducing stable and uniform bubbles. The high volcanic ash active components can also reduce the amount of cement while improving the strength of the crack-resistant concrete, and play the role of air entrainment and foam stabilization and "reducing glue and strengthening". In addition, due to the synergistic effect of the water reducer and the air entraining agent, stable and uniform bubbles can be introduced to play the role of air entrainment and foam stabilization, and the ultrafine fly ash has a stronger "ball effect". Therefore, under the multiple effects of each component and by adopting the preparation method of the present invention to prepare the concrete composite additive, the concrete composite additive can significantly improve the working performance of the concrete. In addition, through the effects of nano-silicon dioxide, ultrafine fly ash and hydraulic lime, the strength performance of the concrete can be improved while reducing the amount of cement, and the cost of raw materials can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] By describing the embodiments of the present application in more detail in conjunction with the accompanying drawings, the above and other purposes, features and advantages of the present application will become more apparent. The accompanying drawings are used to provide a further understanding of the embodiments of the present application and constitute a part of the specification. Together with the embodiments of the present application, they are used to explain the present application and do not constitute a limitation of the present application. In the accompanying drawings, the same reference numerals generally represent the same components or steps. Figure 1 This is a flow chart for the preparation of anti-cracking and anti-seepage composite additives. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0026] The raw materials or additives used in the embodiments of the present invention can be purchased or prepared by oneself.
[0027] An embodiment of the present invention provides a concrete composite additive for crack resistance, and the concrete composite additive specifically includes the following components in parts by weight:
[0028] Deionized water: 100 parts;
[0029] Polymer monomer: 50-80 parts;
[0030] Modified polycarboxylic acid water reducer: 5-25 parts;
[0031] Air entraining agent: 10-20 parts;
[0032] Nano silicon dioxide: 5-15 parts;
[0033] Ultrafine fly ash: 10-15 parts;
[0034] Emulsifier: 5-8 parts;
[0035] Tackifier: 3-6 parts;
[0036] Urea: 2-4 parts;
[0037] Hydraulic lime: 2-4 parts;
[0038] Among them, the polymer monomer is at least one of butyl methacrylate and hydroxyethyl methacrylate; the air entraining agent is sodium dodecylbenzene sulfonate, which has the characteristic of uniformly introducing bubbles; the nano-silicon dioxide has high volcanic ash activity, can significantly replace cement to participate in the hydration reaction, reduce the amount of cement, and improve the strength of concrete, playing the role of "reducing glue and strengthening"; the ultra-fine fly ash plays a ball effect to improve the fluidity of concrete, improve its working performance, and has high volcanic ash activity, which can improve the strength performance of concrete, and play the role of "reducing glue and strengthening"; the hydraulic lime provides calcium ions for admixtures, nano-silicon dioxide and ultra-fine fly ash, promotes the formation of hydration products, and is beneficial to the formation and development of concrete strength; the viscosity enhancer is polyacrylamide, which can increase viscosity and stabilize bubbles, and at the same time improve the working performance of concrete; the urea is used to reduce the freezing temperature of concrete, which is convenient for construction in cold areas.
[0039] The embodiment of the present invention also provides a method for preparing the above concrete composite additive, which specifically comprises:
[0040] After adding the emulsifier to deionized water and heating it to 30-40°C, the polymer monomer and the viscosity enhancer are added and stirred evenly, and then heated to 55-65°C, the water reducer, air entraining agent, nano-silicon dioxide, ultrafine fly ash and hydrated lime are added and stirred evenly, and then cooled to room temperature to obtain a concrete composite additive for crack resistance. 6. The preparation method of the concrete composite additive according to claim 5 is characterized in that the polymer monomer is added twice, and the initial addition amount is 20-40%.
[0041] The stirring time after adding the polymer monomer and the viscosity enhancer is 1-2 hours; the stirring time after adding the water reducer, the air entraining agent, the nano-silicon dioxide, the ultrafine fly ash and the hydrated lime is 2.5-3.5 hours.
[0042] The following are specific embodiments
[0043] Example 1
[0044] The concrete composite additive for crack resistance provided in Example 1 of the present invention specifically includes the following components in parts by weight: 100 parts of deionized water, 50 parts of polymer monomer, 5 parts of modified polycarboxylic acid water reducer, 5 parts of air entraining agent, 5 parts of nano-silica, 5 parts of ultrafine fly ash, 5 parts of emulsifier, 3 parts of viscosity enhancer, 2 parts of urea, and 2 parts of hydraulic lime.
[0045] In addition, the preparation method of the above-mentioned concrete composite additive for crack resistance provided in Example 1 of the present invention is specifically as follows:
[0046] The emulsifier is added into deionized water and heated to 30-40°C, and then the macromolecular polymer and the viscosity enhancer are added and stirred for 1-2 hours, and then the mixture is heated to 55-65°C, and then the water reducer, the air entraining agent, the nano-silicon dioxide and the ultrafine fly ash are added and stirred for 2.5-3.5 hours, and then the mixture is cooled to room temperature, and then urea and hydraulic lime are added and stirred for 2 hours to obtain the composite admixture.
[0047] In addition, the concrete composite additive obtained in Example 1 of the present invention is added to concrete, and the components of the concrete include, by weight: cement: 190 parts, Class I fly ash: 90 parts, silica fume: 105 parts, coarse aggregate: 1080 parts, fine aggregate: 790 parts, composite admixture: 6.8 parts, 15wt% polyethylene glycol aqueous solution: 120 parts, regenerated fiber: 11.5 parts, and water: 180 parts.
[0048] Example 2
[0049] The concrete composite additive for crack resistance provided in Example 2 of the present invention specifically includes the following components in parts by weight: 100 parts of deionized water, 60 parts of polymer monomer, 10 parts of modified polycarboxylic acid water reducer, 15 parts of air entraining agent, 8 parts of nano-silica, 10 parts of ultrafine fly ash, 6 parts of emulsifier, 4 parts of viscosity enhancer, 3 parts of urea, and 3 parts of hydraulic lime.
[0050] In addition, the preparation method of the above-mentioned concrete composite additive for crack resistance provided in Example 2 of the present invention is the same as that in Example 1, and will not be repeated herein.
[0051] In addition, the anti-cracking concrete composite additive obtained in Example 2 of the present invention is added to concrete, and the components of the concrete include, by weight: cement: 190 parts, Class I fly ash: 90 parts, silica fume: 105 parts, coarse aggregate: 1080 parts, fine aggregate: 790 parts, composite admixture: 6.6 parts, 15wt% polyethylene glycol aqueous solution: 120 parts, regenerated fiber: 11.5 parts, and water: 180 parts.
[0052] Example 3
[0053] The concrete composite additive for crack resistance provided in Example 3 of the present invention specifically includes the following components in parts by weight: 100 parts of deionized water, 70 parts of polymer monomer, 18 parts of modified polycarboxylic acid water reducer, 18 parts of air entraining agent, 10 parts of nano-silica, 13 parts of ultrafine fly ash, 8 parts of emulsifier, 5 parts of viscosity enhancer, 3 parts of urea, and 4 parts of hydraulic lime.
[0054] In addition, the preparation method of the above-mentioned concrete composite additive for crack resistance provided in Example 3 of the present invention is the same as that in Example 1, and will not be repeated herein.
[0055] In addition, the anti-cracking concrete composite additive obtained in Example 3 of the present invention is added to concrete, and the components of the concrete include, by weight: cement: 190 parts, Class I fly ash: 90 parts, silica fume: 105 parts, coarse aggregate: 1080 parts, fine aggregate: 790 parts, composite admixture: 6.3 parts, 15wt% polyethylene glycol aqueous solution: 120 parts, regenerated fiber: 11.5 parts, and water: 180 parts.
[0056] Example 4
[0057] The concrete composite additive for crack resistance provided in Example 4 of the present invention specifically includes the following components in parts by weight: 100 parts of deionized water, 80 parts of polymer monomer, 25 parts of modified polycarboxylic acid water reducer, 20 parts of air entraining agent, 15 parts of nano-silica, 15 parts of ultrafine fly ash, 5 parts of emulsifier, 6 parts of viscosity enhancer, 4 parts of urea, and 4 parts of hydraulic lime.
[0058] In addition, the preparation method of the above-mentioned concrete composite additive for crack resistance provided in Example 4 of the present invention is the same as that in Example 1 and will not be repeated herein.
[0059] In addition, the anti-cracking concrete composite additive obtained in Example 3 of the present invention is added to concrete, and the components of the concrete include, by weight: cement: 190 parts, Class I fly ash: 90 parts, silica fume: 105 parts, coarse aggregate: 1080 parts, fine aggregate: 790 parts, composite admixture: 6.1 parts, 15wt% polyethylene glycol aqueous solution: 120 parts, regenerated fiber: 11.5 parts, and water: 180 parts.
[0060] Figure 1 The preparation flow chart of the anti-cracking and anti-seepage composite additive mainly includes: adding the emulsifier to deionized water and heating it to 30-40°C, adding the viscosity enhancer and adding the polymer emulsion twice, stirring evenly, and the stirring time after adding the polymer monomer and the viscosity enhancer is 1-2h. Then, heating to 55-65°C, adding the water reducer, air entraining agent, nano-silica, ultrafine fly ash and hydrated lime, stirring for 2.5-3.5h, and then cooling to room temperature to obtain the composite additive for anti-cracking concrete.
[0061] Performance testing
[0062] Slump test: Test the slump of concrete in accordance with the Test Procedure for Cement and Cement Concrete for Highway Engineering (JTG E30-2005).
[0063] Mechanical properties test: The strength of concrete was tested in accordance with the "Testing Procedures for Cement and Cement Concrete for Highway Engineering" (JTG E30-2005). Concrete specimens of 100mm×100mm×100mm and 100mm×100mm×400mm were formed according to the procedure. After curing for 2 days, the specimens were demoulded and placed in a standard curing room for curing for 28 days before strength testing.
[0064] Crack resistance test: The crack resistance test is carried out using the ring constraint method. The inner diameter of the ring constraint device is 30.4cm, the outer diameter is 45.6cm, and the height is 16cm. Four crack inducers are added to the inner steel ring. The setting of crack inducers can accelerate the cracking process of concrete and significantly reduce the test cycle.
[0065] In order to verify the anti-cracking performance of the composite additive obtained in the present invention, the anti-cracking concrete added with the composite additive in Implementation 1-Example 4 is subjected to a working performance test and a mechanical performance test, and its anti-cracking performance is tested by a ring restraint device. The specific test performance is shown in the table:
[0066] Table 1 Test results of crack resistance of concrete composite additives obtained in Examples 1-4
[0067]
[0068] By combining the comparative examples with the analysis in Table 1, it can be seen that the slump, strength and crack resistance of crack-resistant concrete can be effectively improved by adding composite additives. The improvement in working performance is mainly attributed to the significant increase in the content of air entraining agent and the increase in the content of ultrafine fly ash, which introduces a large number of uniformly distributed, closed and stable bubbles into the concrete. In addition, the "ball effect" in the system is further enhanced, thereby significantly improving the working performance of concrete.
[0069] By combining Example 1 with Example 4 and Table 1, it can be seen that the improvement in mechanical properties is mainly attributed to the increase in the content of ultrafine fly ash and nano-silicon dioxide. Nano-silicon dioxide with high volcanic ash activity participates in the hydration reaction and promotes the decomposition of the outer shell of fly ash particles, prompting it to release the active SiO2 and Al2O3 components inside, which further promotes the formation and development of concrete strength and shows higher mechanical properties.
[0070] By combining the analysis of Example 1, Example 3 and Example 4 and Table 1, it can be seen that the improvement in crack resistance is mainly attributed to the significant improvement in the density of the concrete structure. The highly active mineral admixture provides sufficient calcium hydroxide through hydraulic lime to fully participate in the hydration reaction inside the concrete, thereby generating a sufficient amount of gelling material (CSH gel) for the concrete system, thereby significantly improving the density of the system and improving the crack resistance.
[0071] In summary, by applying the concrete composite additive of the present invention to concrete, the working performance of the crack-resistant concrete can be improved by reducing the water-cement ratio and introducing stable and uniform bubbles. The high volcanic ash active component can also reduce the amount of cement while improving the strength of the crack-resistant concrete, and play the role of air entrainment and foam stabilization and "reducing glue and strengthening". In addition, due to the synergistic effect of the water reducer and the air entraining agent, stable and uniform bubbles can be introduced to play the role of air entrainment and foam stabilization. At the same time, the ultrafine fly ash has a stronger "ball effect". Therefore, under the multiple effects of each component and by adopting the preparation method of the present invention to prepare the concrete composite additive, the concrete composite additive can significantly improve the working performance of the concrete. In addition, through the effects of nano-silica, ultrafine fly ash and hydraulic lime, the strength performance of the concrete can be improved while reducing the amount of cement, thereby reducing the cost of raw materials.
[0072] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A concrete composite additive for crack resistance, characterized in that: The concrete composite additive specifically comprises the following components in parts by weight: deionized water: 100 parts; Polymer monomer: 50-80 parts; Modified polycarboxylic acid water reducer: 5-25 parts; Air entraining agent: 10-20 parts; Nano silicon dioxide: 5-15 parts; Ultrafine fly ash: 10-15 parts; Emulsifier: 5-8 parts; Tackifier: 3-6 parts; Urea: 2-4 parts; Hydraulic lime: 2-4 parts.
2. The concrete composite additive according to claim 1, characterized in that: The polymer monomer is at least one of butyl methacrylate and hydroxyethyl methacrylate.
3. The concrete composite additive according to claim 1, characterized in that: The air entraining agent is sodium dodecylbenzene sulfonate.
4. The concrete composite additive according to claim 1, characterized in that: The tackifier is polyacrylamide.
5. The method for preparing the composite concrete additive according to any one of claims 1 to 4, characterized in that: The method is as follows: The emulsifier is added to deionized water and heated to 30-40°C, and then the polymer monomer and viscosity enhancer are added and stirred evenly. Then, the mixture is heated to 55-65°C, and then a water reducer, an air entraining agent, nano-silica, ultrafine fly ash and hydrated lime are added and stirred evenly, and then cooled to room temperature to obtain a concrete composite additive for crack resistance.
6. The method for preparing the composite concrete additive according to claim 5, characterized in that: The polymer monomer is added in two times, with the initial addition amount being 20-40%.
7. The method for preparing the composite concrete additive according to claim 5, characterized in that: The stirring time after adding the polymer monomer and the tackifier is 1-2 hours.
8. The method for preparing the composite concrete additive according to claim 5, characterized in that: The stirring time after adding water reducing agent, air entraining agent, nano-silica, ultrafine fly ash and hydrated lime is 2.5-3.5h.
Citation Information
Patent Citations
Anti-crack concrete
CN105601186A
Anti-crack concrete admixture
CN110482899A
Preparation method of macromolecular anti-cracking and anti-seepage mortar modifier
CN111056763A
Compact anti-cracking waterproof agent capable of inhibiting early cracking of concrete and preparation method of dense anti-cracking waterproof agent
CN112851191A
Modified micro-nano composite superfine admixture high-durability anti-crack concrete and preparation method thereof
CN113998960A
Cited By
Self-leveling anti-dispersion underwater bottom sealing material and preparation method thereof
CN119528527A