Multi-component anti-crack cement material and manufacturing process thereof

By using brûlite fiber modified material and sulfonic acid crosslinked cellulose-based gel agent in cement material, the crack problem during the drying process of cement material is solved, the compressive strength and crack resistance are improved, and the porosity is reduced. Internal stress significantly improves the stability and safety of cement components.

CN118930177APending Publication Date: 2024-11-12ZHEJIANG XINDU CEMENT CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411091873.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing cement materials are prone to cracks during drying, which affects the safety and aesthetics of the building structure. The large aggregate particle size leads to an increase in pores during the mixing process, affecting the mechanical properties and crack resistance.

Method used

Using a multi-component anti-cracking cement material process, including the use of brevice fiber modified material and sulfonic acid crosslinking cellulose-based gel agent, prepared by brevice fiber surface modification and cellulose crosslinking to form a network binding mode and Continuous hydration effect, reduce porosity and internal stress, and enhance compressive strength and crack resistance.

Benefits of technology

Effectively reduce the internal porosity of cement components, enhance mechanical properties and crack resistance, avoid cracking caused by drying and shrinking, and significantly improve the compressive strength and crack resistance of cement materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930177A_ABST
    Figure CN118930177A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of building materials, and discloses a multi-component anti-crack cement material and a manufacturing process thereof.The cement material is formed by taking ordinary Portland cement, gravel, fine sand and the like as main components and fly ash, a brucite fiber modified material, a gelling agent and the like as additives through wet mixing, wherein the brucite fiber modified material can be riveted in the cement material to form a strong constraint and traction effect, so that the mechanical property and the crack resistance of the cement material are effectively enhanced, and the gel has extremely strong hydrophilicity, can absorb a large amount of water in the initial hydration stage of the cement material and store the water, and releases the water under the action of pressure difference in the later hydration stage, so that the cement material is prevented from cracking. A continuous hydration effect is generated, so that the internal stress generated by drying shrinkage of the cement material is reduced, and the cracking phenomenon caused by too high shrinkage rate of the cement material can be avoided, so that the anti-cracking performance of the cement material is improved from different angles by cooperating with the brucite fiber modified material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a multi-component anti-cracking cement material and a manufacturing process thereof. Background Art

[0002] With the continuous improvement and upgrading of infrastructure, the consumption of building materials has gradually increased. As an indispensable building material in civil engineering, cement's performance directly affects the stability and durability of building structures. However, due to the phenomenon of self-shrinkage and drying shrinkage during the drying process of cement, these phenomena will cause cracks in cement components. The cracks will gradually expand during the use of cement components. When the crack width exceeds a certain limit, it will not only affect the aesthetics of the building, but also seriously affect the bearing capacity of the cement components, thus posing a serious threat to the structural safety of the building. Therefore, how to take effective measures to reduce the drying shrinkage of cement and improve the crack resistance of cement has always been a research hotspot.

[0003] At present, the cracking problem of cement is mainly improved by adding additives such as anti-cracking agents and shrinkage reducing agents. For example, the invention patent with application number CN201510827777.X discloses a low shrinkage and crack-resistant concrete, which is to achieve a super-superposition effect by adding a shrinkage reducing agent, and combining components such as rice husk ash, corundum powder and corundum, and effectively improve the anti-cracking performance of cement by adjusting the mass ratio between the components. In addition, by adding anti-cracking fibers, the anti-cracking performance of cement can also be improved through the restraint and restriction of fibers. However, the aggregate particle size in cement is relatively large, and during the mixing process, it is easy to produce large pores between the fibers. The presence of pores will also have a negative impact on the mechanical properties and anti-cracking performance of cement.

[0004] Based on this, the present invention provides a multi-component anti-cracking cement material, which can solve the problems existing in the prior art. Summary of the invention

[0005] In order to solve the problems mentioned in the background technology, an object of the present invention is to provide a and a manufacturing process thereof.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A manufacturing process of a multi-component anti-cracking cement material, the anti-cracking cement material comprising the following raw materials measured by weight: 60-80 parts of ordinary Portland cement, 15-30 parts of fly ash, 3-6 parts of brucite fiber modified material, 100-150 parts of crushed stone, 50-60 parts of fine sand, 2-4.5 parts of gelling agent, 4-8 parts of water reducing agent, and 80-100 parts of water;

[0008] The manufacturing process comprises the following steps:

[0009] Step 1: Prepare the ingredients

[0010] Weigh the raw materials of each component according to the above weight parts and set aside;

[0011] Step 2: Mixing

[0012] First, put silicate cement, fly ash, brucite fiber modified material, coarse aggregate, fine aggregate and gelling agent into a mixer, mix them at a speed of 1000-1500r / min for 10-20min, then adjust the speed to 500-600r / min, add water reducer and water into the mixer, continue stirring for 5-15min, discharge the materials, and obtain anti-cracking cement material.

[0013] As a further embodiment of the present invention, the method for preparing the modified brucite fiber material comprises the following steps:

[0014] Step A: Surface modification of brucite fiber

[0015] The brucite fiber is added to toluene and mixed into a uniform dispersion, and then the diisocyanate bridge is added to the dispersion. After the addition is completed, the temperature is gradually increased to 80-90° C., and after keeping the temperature for 3-6 hours, the material is collected by centrifugation to obtain a brucite fiber intermediate material;

[0016] Step B: Preparation of brucite modified material

[0017] The brucite fiber intermediate material is added to dimethyl sulfoxide, and after being evenly dispersed, agarose is added, nitrogen is passed through for protection, and then the temperature is controlled at 60-70°C, and a tin metal catalyst is added. After the addition is completed, the mixture is stirred for 6-9 hours at a temperature of 100-150°C, the material is discharged after cooling, and the solid material is collected by centrifugation to obtain the brucite fiber modified material.

[0018] As a further embodiment of the present invention, in step A, the diisocyanate bridge is selected from any one of toluene-2,4-diisocyanate, isophorone diisocyanate or diphenylmethane diisocyanate.

[0019] As a further embodiment of the present invention, in step B, the mass ratio of the brucite fiber intermediate material to agarose is 1:4-6.

[0020] As a further embodiment of the present invention, in step B, the tin metal catalyst is selected from any one of stannous octoate, dibutyltin dilaurate or dibutyltin diacetate.

[0021] As a further embodiment of the present invention, the preparation method of the gel comprises the following steps:

[0022] Step ①, preparation of carboxymethyl cellulose

[0023] Add cellulose to sodium hydroxide aqueous solution, stir mechanically to mix, then add chloroacetic acid, after adding, keep warm at 50-60°C for 8-12h, discharge, and obtain carboxymethyl cellulose;

[0024] Step 2: Preparation of gel

[0025] Add carboxymethyl cellulose to N,N-dimethylformamide, shake well, then add 4-dimethylaminopyridine and dicyclohexylcarbodiimide, stir at room temperature for 20-40 minutes to form a pre-reaction liquid, then add the sulfonic acid cross-linking agent to the pre-reaction liquid, continue to stir at room temperature for 6-9 hours, stop stirring, pour into a mold and let stand to form a gel, then put it in a freeze dryer, treat it at -20°C for 12-24 hours, discharge it, grind it, and prepare a gel.

[0026] As a further solution of the present invention, in step ①, the mass fraction of the sodium hydroxide is 20-30%.

[0027] As a further embodiment of the present invention, in step ②, the sulfonic acid cross-linking agent is N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid.

[0028] As a further embodiment of the present invention, the water reducer is a naphthalene-based water reducer or a polycarboxylic acid water reducer.

[0029] A multi-component anti-cracking cement material is prepared by adopting the above manufacturing process.

[0030] Beneficial effects of the present invention:

[0031] (1) The present invention obtains modified brucite fiber material by modifying the surface of brucite fiber with agarose, a macromolecular substance, as an anti-cracking additive. Since agarose contains a large number of hydroxyl groups in its structure, it can electrostatically attract calcium ions in cement particles, so that a large number of cement particles are adsorbed on the surface of brucite fiber, which can effectively fill the gap between aggregate and brucite fiber, thereby reducing the internal porosity of cement components, which is beneficial to improving the mechanical properties of cement components such as compressive strength. In addition, the presence of agarose molecular chains can play a role similar to that of capillary fibers, extending to various positions of cement materials, so that a network bonding mode can be formed between brucite fiber and cement materials, so that brucite fiber can be riveted in cement materials, forming a strong restraining and pulling effect, thereby effectively enhancing the mechanical properties and anti-cracking performance of cement materials.

[0032] (2) The present invention uses a sulfonic acid crosslinking agent to crosslink cellulose, and then uses freeze-drying to prepare a cellulose-based aerogel material containing a large number of sulfonic acid groups in its structure. Since the sulfonic acid group has strong hydrophilicity and is combined with the special structure of the cellulose-based aerogel material, it can absorb a large amount of water in the early stage of hydration of the cement material and store it. Later, under the action of pressure difference, the water is released, thereby producing a continuous hydration effect during the drying and shrinking process of the cement, thereby reducing the internal stress generated by the drying and shrinking of the cement material, and avoiding the cracking phenomenon caused by the excessive shrinkage rate of the cement material, thereby synergizing with the brucite fiber modified material to improve the crack resistance of the cement material from different angles.

[0033] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0035] Figure 1 This is a scanning electron micrograph of the gel. DETAILED DESCRIPTION

[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The silicate cement used in the following examples and comparative examples is 42.5R type ordinary silicate cement; the fly ash is selected as Class II fly ash; the crushed stone is selected as crushed stone with a particle size of less than 5 mm; the fine sand is selected as river sand with a particle size of less than 2 mm, and the water reducer is selected as polycarboxylic acid water reducer.

[0038] Example 1

[0039] A multi-component anti-cracking cement material, comprising the following raw materials measured by weight: 60 parts of ordinary Portland cement, 15 parts of fly ash, 3 parts of brucite fiber modified material, 100 parts of crushed stone, 50 parts of fine sand, 2 parts of gelling agent, 4 parts of water reducing agent, and 80 parts of water;

[0040] The manufacturing process of the anti-cracking cement material comprises the following steps:

[0041] Step 1: Prepare the ingredients

[0042] Weigh the raw materials of each component according to the above weight parts and set aside;

[0043] Step 2: Mixing

[0044] First, put silicate cement, fly ash, brucite fiber modified material, coarse aggregate, fine aggregate and gelling agent into a mixer, mix at a speed of 1000r / min for 20min, then adjust the speed to 500r / min, add water reducer and water into the mixer, continue stirring for 15min, discharge the material, and obtain anti-cracking cement material.

[0045] Example 2

[0046] A multi-component anti-cracking cement material, comprising the following raw materials measured by weight: 70 parts of ordinary Portland cement, 25 parts of fly ash, 5 parts of brucite fiber modified material, 120 parts of crushed stone, 55 parts of fine sand, 4 parts of gelling agent, 6 parts of water reducing agent, and 95 parts of water;

[0047] The manufacturing process of the anti-cracking cement material comprises the following steps:

[0048] Step 1: Prepare the ingredients

[0049] Weigh the raw materials of each component according to the above weight parts and set aside;

[0050] Step 2: Mixing

[0051] First, silicate cement, fly ash, brucite fiber modified material, coarse aggregate, fine aggregate and gelling agent are put into a mixer and mixed at a speed of 1200 r / min for 15 minutes. Then the speed is adjusted to 600 r / min, and the water reducer and water are added to the mixer. The mixing is continued for 10 minutes and the material is discharged to obtain the crack-resistant cement material.

[0052] Example 3

[0053] A multi-component anti-cracking cement material, comprising the following raw materials measured by weight: 80 parts of ordinary Portland cement, 30 parts of fly ash, 6 parts of brucite fiber modified material, 150 parts of crushed stone, 60 parts of fine sand, 4.5 parts of gelling agent, 8 parts of water reducing agent, and 100 parts of water;

[0054] The manufacturing process of the anti-cracking cement material comprises the following steps:

[0055] Step 1: Prepare the ingredients

[0056] Weigh the raw materials of each component according to the above weight parts and set aside;

[0057] Step 2: Mixing

[0058] First, put silicate cement, fly ash, brucite fiber modified material, coarse aggregate, fine aggregate and gelling agent into a mixer, mix at a speed of 1500r / min for 10min, then adjust the speed to 600r / min, add water reducer and water into the mixer, continue stirring for 5min, discharge the material, and obtain anti-cracking cement material.

[0059] Comparative Example 1

[0060] A multi-component anti-cracking cement material, comprising the following raw materials measured by weight: 70 parts of ordinary Portland cement, 25 parts of fly ash, 5 parts of brucite fiber, 120 parts of crushed stone, 55 parts of fine sand, 4 parts of gelling agent, 6 parts of water reducing agent, and 95 parts of water;

[0061] The manufacturing process of the anti-cracking cement material comprises the following steps:

[0062] Step 1: Prepare the ingredients

[0063] Weigh the raw materials of each component according to the above weight parts and set aside;

[0064] Step 2: Mixing

[0065] First, put silicate cement, fly ash, brucite fiber, coarse aggregate, fine aggregate and gelling agent into a mixer, mix at a speed of 1200r / min for 15min, then adjust the speed to 600r / min, add water reducer and water into the mixer, continue stirring for 10min, discharge the material, and obtain anti-cracking cement material.

[0066] Comparative Example 2

[0067] A multi-component anti-cracking cement material, comprising the following raw materials measured by weight: 70 parts of ordinary Portland cement, 25 parts of fly ash, 120 parts of crushed stone, 55 parts of fine sand, 4 parts of gelling agent, 6 parts of water reducing agent, and 95 parts of water;

[0068] The manufacturing process of the anti-cracking cement material comprises the following steps:

[0069] Step 1: Prepare the ingredients

[0070] Weigh the raw materials of each component according to the above weight parts and set aside;

[0071] Step 2: Mixing

[0072] First, put silicate cement, fly ash, coarse aggregate, fine aggregate and gelling agent into a mixer, mix at a speed of 1200r / min for 15 minutes, then adjust the speed to 600r / min, add water reducer and water into the mixer, continue stirring for 10 minutes, discharge the material, and obtain anti-cracking cement material.

[0073] Comparative Example 3

[0074] A multi-component anti-cracking cement material, comprising the following raw materials measured by weight: 70 parts of ordinary Portland cement, 25 parts of fly ash, 5 parts of brucite fiber modified material, 120 parts of crushed stone, 55 parts of fine sand, 6 parts of water reducer, and 95 parts of water;

[0075] The manufacturing process of the anti-cracking cement material comprises the following steps:

[0076] Step 1: Prepare the ingredients

[0077] Weigh the raw materials of each component according to the above weight parts and set aside;

[0078] Step 2: Mixing

[0079] First, put silicate cement, fly ash, brucite fiber modified material, coarse aggregate and fine aggregate into a mixer, mix them at a speed of 1200r / min for 15 minutes, then adjust the speed to 600r / min, add water reducer and water into the mixer, continue stirring for 10 minutes, discharge the material, and obtain anti-cracking cement material.

[0080] The brucite fiber modified materials in the above examples and comparative examples were prepared by the following method:

[0081] Step A: Surface modification of brucite fiber

[0082] 5 g of brucite fiber was added to toluene and mixed into a uniform dispersion, and then 8.5 g of toluene-2,4-diisocyanate was added to the dispersion. After the addition was completed, the temperature was gradually raised to 85° C., and after keeping the temperature for 4 hours, the material was collected by centrifugation to obtain a brucite fiber intermediate material;

[0083] The hydrochloric acid-di-n-butylamine method was used to titrate the brucite fiber intermediate material. 0.2g of the brucite fiber intermediate material sample was taken and titrated with a 0.5mol / L hydrochloric acid standard solution. The isocyanate content of the brucite fiber intermediate material was measured to be 9.817%.

[0084] Step B: Preparation of brucite modified material

[0085] 3.6 g of brucite fiber intermediate material was added to dimethyl sulfoxide, and after uniform dispersion, 15 g of agarose was added, and nitrogen was passed through for protection. Then the temperature was controlled at 65°C, and 0.05 g of dibutyltin dilaurate was added. After the addition, the mixture was stirred for 8 h at a constant temperature, the temperature was lowered and the material was discharged. The solid material was collected by centrifugation to obtain a brucite fiber modified material.

[0086] The same method was used to test the isocyanate group content of the brucite fiber modified material, and the result was 1.524%. This was due to the reaction between the isocyanate groups of the brucite fiber intermediate material and the substituted hydroxyl groups in the agarose structure, resulting in a large amount of consumption.

[0087] It can be reasonably speculated that the brucite fiber surface contains hydroxyl groups, which can react with the isocyanate group at one end of the toluene-2,4-diisocyanate structure to achieve the purpose of modifying the isocyanate group on the brucite fiber surface and obtain the brucite intermediate material. Then, the high reactivity of the isocyanate group is utilized to further react with the hydroxyl group in the agarose structure to carry out amine esterification, thereby modifying the agarose macromolecule on the brucite fiber surface.

[0088] The gels in the above examples and comparative examples were prepared by the following method:

[0089] Step ①, preparation of carboxymethyl cellulose

[0090] 1.5 g of cellulose was added to 30 mL of 25% sodium hydroxide aqueous solution, and mechanically stirred to mix, followed by adding 1.2 g of chloroacetic acid. After the addition, the mixture was kept at 55° C. for 9 h, and the material was discharged to obtain carboxymethyl cellulose.

[0091] Step 2: Preparation of gel

[0092] Add 0.8 g of carboxymethyl cellulose to N,N-dimethylformamide, shake well, then add 0.1 g of 4-dimethylaminopyridine and 0.2 g of dicyclohexylcarbodiimide, stir at room temperature for 30 min to form a pre-reaction liquid, then add 0.5 g of N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid to the pre-reaction liquid, continue stirring at room temperature for 8 h, stop stirring, pour into a mold and let stand to form a gel, then put it in a freeze dryer, treat it at -20 ° C for 24 h, discharge the material, grind and crush to obtain a gel.

[0093] The percentage of organic elements in the gelling agent was tested using a TQ-3 organic element analyzer. The test results showed that the percentage of carbon element was 43.97%, the percentage of sulfur element was 4.11%, and the percentage of nitrogen element was 1.76%.

[0094] Figure 1 This is a scanning electron microscope image of the gelling agent. It can be observed from the image that the gelling agent contains a rich and uniform pore structure, which can absorb and store a large amount of water, and release the water under the pressure difference caused by the subsequent cement shrinkage, thereby producing a continuous hydration effect during the cement drying and shrinkage process.

[0095] Test Case

[0096] According to standard JGJ / T 70-2009, mechanical properties test was carried out;

[0097] According to the standard JC / T 951-2005, cracking performance test is carried out;

[0098] The test results are recorded in the following table:

[0099] 28d compressive strength / MPa Cracking index(mm) Example 1 78.4 144.8 Example 2 79.1 143.5 Example 3 78.9 144.4 Comparative Example 1 70.4 161.9 Comparative Example 2 57.8 182.1 Comparative Example 3 75.6 159.0

[0100] Analysis of the test results shows that the cement prepared by adding brucite fiber modified material and gelling agent as raw materials obviously shows better mechanical strength and crack resistance. After replacing the brucite fiber modified material with brucite fiber, due to the large gap between brucite fiber and aggregate, the advantages of brucite fiber are difficult to fully play, so the mechanical strength and crack resistance are reduced. After directly removing the brucite fiber, its restraint and traction effect cannot be utilized, and the mechanical properties and crack resistance of the cement are greatly reduced. In addition, after removing the aerogel material, the drying shrinkage of the cement material is too fast, resulting in poor crack resistance.

[0101] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.

Claims

1. A process for manufacturing a multi-component anti-cracking cement material, characterized in that: The anti-cracking cement material includes the following raw materials measured by weight: 60-80 parts of ordinary Portland cement, 15-30 parts of fly ash, 3-6 parts of brucite fiber modified material, 100-150 parts of crushed stone, 50-60 parts of fine sand, 2-4.5 parts of gelling agent, 4-8 parts of water reducing agent, and 80-100 parts of water; The manufacturing process comprises the following steps: Step 1: Prepare the ingredients Weigh the raw materials of each component according to the above weight parts and set aside; Step 2: Mixing First, put silicate cement, fly ash, brucite fiber modified material, coarse aggregate, fine aggregate and gelling agent into a mixer, mix them at a speed of 1000-1500r / min for 10-20min, then adjust the speed to 500-600r / min, add water reducer and water into the mixer, continue stirring for 5-15min, discharge the materials, and obtain anti-cracking cement material.

2. The manufacturing process of a multi-component anti-cracking cement material according to claim 1, characterized in that: The preparation method of the modified brucite fiber material comprises the following steps: Step A: Surface modification of brucite fiber Using diisocyanate bridge body and toluene as medium, brucite fiber is surface modified at 80-90°C to obtain brucite fiber intermediate material; Step B: Preparation of brucite modified material The brucite fiber intermediate material is added to dimethyl sulfoxide, and after being evenly dispersed, agarose is added, nitrogen is passed through for protection, and then the temperature is controlled at 60-70°C, and a tin metal catalyst is added. After the addition is completed, the mixture is stirred for 6-9 hours at a temperature of 100-150°C, the material is discharged after cooling, and the solid material is collected by centrifugation to obtain the brucite fiber modified material.

3. The manufacturing process of a multi-component anti-cracking cement material according to claim 2, characterized in that: In step A, the diisocyanate bridge is selected from any one of toluene-2,4-diisocyanate, isophorone diisocyanate or diphenylmethane diisocyanate.

4. The manufacturing process of a multi-component anti-cracking cement material according to claim 2, characterized in that: In step B, the mass ratio of the brucite fiber intermediate material to agarose is 1:4-6.

5. The manufacturing process of a multi-component anti-cracking cement material according to claim 2, characterized in that: In step B, the tin metal catalyst is selected from any one of stannous octoate, dibutyltin dilaurate or dibutyltin diacetate.

6. The manufacturing process of a multi-component anti-cracking cement material according to claim 1, characterized in that: The preparation method of the gel comprises the following steps: Step ①, preparation of carboxymethyl cellulose Using chloroacetic acid as a modifier, cellulose is substituted and modified to obtain carboxymethyl cellulose; Step 2: Preparation of gel Add carboxymethyl cellulose to N,N-dimethylformamide, shake well, then add 4-dimethylaminopyridine and dicyclohexylcarbodiimide, stir at room temperature for 20-40 minutes to form a pre-reaction liquid, then add the sulfonic acid cross-linking agent to the pre-reaction liquid, continue to stir at room temperature for 6-9 hours, stop stirring, pour into a mold and let stand to form a gel, then put it in a freeze dryer, treat it at -20°C for 12-24 hours, discharge it, grind it, and prepare a gel.

7. The manufacturing process of a multi-component anti-cracking cement material according to claim 2, characterized in that: In step ①, the mass fraction of the sodium hydroxide is 20-30%.

8. The manufacturing process of a multi-component anti-cracking cement material according to claim 2, characterized in that: In step ②, the sulfonic acid cross-linking agent is N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid.

9. The manufacturing process of a multi-component anti-cracking cement material according to claim 1, characterized in that: The water reducer is a naphthalene-based water reducer or a polycarboxylic acid water reducer.

10. A multi-component anti-cracking cement material, characterized in that: The method is prepared by the manufacturing process as described in any one of claims 1 to 9.

Citation Information

Cited By

  • Portland cement-based multi-component concrete and preparation method thereof

    CN119613059A