High-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion as well as preparation method and application of high-entropy rare earth silicate ceramic material
By optimizing the ratio of rare earth elements, high-entropy rare earth silicate ceramic materials, and using wet ball milling and sintering processes, it significantly improves its anti-CMAS corrosion performance at high temperatures, solves the problem of insufficient performance of existing materials, and is suitable for aerospace field.
Patent Information
- Application Number
- CN202411012994.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-26
AI Technical Summary
The existing high-entropy rare earth silicate ceramic materials still have poor performance on CMAS corrosion at high temperatures and cannot fully meet the application requirements in the aerospace field.
The high-entropy rare earth silicate ceramic material with the chemical formula (HoxErxYb0.5-xLu0.5-x)2SiO5 was prepared by wet ball milling and sintering processes, and the proportion of rare earth elements was optimized to improve the corrosion resistance of high-temperature CMAS.
The corrosion depth after 80 hours of CMAS corrosion at 1400°C is only 75μm~88μm, and the corrosion rate is 0.9μm/h~1.1μm/h, which significantly improves the corrosion resistance of high-temperature CMAS, and is simple in process and low in cost. It is suitable for use in the use of Thermal end components of aerospace engines.
Smart Images

Figure CN118930266A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high entropy ceramic materials, and in particular to a high entropy rare earth silicate ceramic material resistant to high temperature CMAS corrosion, and a preparation method and application thereof. Background Art
[0002] High-temperature CMAS corrosion refers to the destruction of thermal barrier / environmental barrier coatings by CaO, MgO, Al2O3 and SiO2 (CMAS for short) at high temperatures. It is one of the main problems faced by the hot end components of aircraft engines (for example, turbine blades, combustion chamber walls, etc.). High-entropy rare earth silicate ceramic materials have the advantages of good high-temperature stability, low thermal conductivity, thermal expansion coefficient matching the SiC matrix, excellent resistance to water and oxygen corrosion, and good resistance to high-temperature CMAS. They are considered to be the best candidate materials for the next generation of thermal barrier / environmental barrier coatings and have very broad application prospects in the aerospace field. However, the high-temperature CMAS corrosion resistance of existing high-entropy rare earth silicate ceramic materials is still not ideal. For example, the high-entropy rare earth silicate ceramic material with the best high-temperature CMAS corrosion resistance reported so far is (Ho 0.25 Yb 0.25 Lu 0.25 Er 0.25 )2SiO5, after CMAS corrosion for 48h at 1400℃, the corrosion depth reached 64μm, and the corrosion rate was 1.3μm / h (High-throughput composition screening of high-entropy rare-earth monosilicates for superior CMAS corrosion resistance up to1873K,Peng Wei,Yiwen Liu,Yang Liu,Lei Zhuang,Hulei Yu,Yanhui Chu.CorrosionScience,235(2024):112172), which is difficult to fully meet the requirements of practical applications, resulting in its application being greatly restricted.
[0003] Therefore, it is of great significance to develop a high-entropy rare earth silicate ceramic material with excellent resistance to high-temperature CMAS corrosion. Summary of the invention
[0004] The object of the present invention is to provide a high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion and a preparation method and application thereof.
[0005] The technical solution adopted by the present invention is:
[0006] A high entropy rare earth silicate ceramic material resistant to high temperature CMAS corrosion, the chemical formula of its composition is (Ho x Er x Yb 0.5-x Lu 0.5-x )2SiO5, wherein x=0.05~0.15 or 0.35~0.45.
[0007] Preferably, the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion has a corrosion depth of 75 μm to 88 μm and a corrosion rate of 0.9 μm / h to 1.1 μm / h after CMAS corrosion for 80 hours at 1400°C.
[0008] A method for preparing the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion as described above comprises the following steps:
[0009] 1) Ho2O3 powder, Er2O3 powder, Yb2O3 powder, Lu2O3 powder and SiO2 powder are weighed according to the stoichiometric ratio, mixed and wet-milled to obtain a mixed powder slurry;
[0010] 2) drying the mixed powder slurry and then calcining it to obtain high entropy rare earth silicate ceramic powder;
[0011] 3) wet-milling and drying the high-entropy rare earth silicate ceramic powder and then forming it to obtain a green body;
[0012] 4) Sintering the green body to obtain a high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion.
[0013] Preferably, the particle size of the Ho2O3 powder in step 1) is 1 μm to 3 μm, and the purity is ≥ 99.9%.
[0014] Preferably, the particle size of the Er2O3 powder in step 1) is 1 μm to 3 μm, and the purity is ≥ 99.9%.
[0015] Preferably, the particle size of the Yb2O3 powder in step 1) is 1 μm to 3 μm, and the purity is ≥ 99.9%.
[0016] Preferably, the particle size of the Lu2O3 powder in step 1) is 1 μm to 3 μm, and the purity is ≥ 99.9%.
[0017] Preferably, the particle size of the SiO2 powder in step 1) is 100nm to 200nm, and the purity is ≥99.9%.
[0018] Preferably, the process parameters of the wet ball milling in step 1) are as follows: the ball milling medium is anhydrous ethanol, the weight ratio of the powder raw material, ZrO2 balls and anhydrous ethanol is 1:1.8~2.2:1.0~1.5, and the ball milling time is 6h~10h.
[0019] Preferably, the ball milling equipment used in the wet ball milling in step 1) is a planetary ball mill.
[0020] Preferably, the specific operation of the calcination in step 2) is as follows: first control the heating rate to be 6°C / min-10°C / min from room temperature (25°C±5°C) to 1400°C-1500°C, then keep it warm for 2h-4h, and then cool it to room temperature with the furnace.
[0021] Preferably, the heating furnace used for the calcination in step 2) is a muffle furnace.
[0022] Preferably, the process parameters of the wet ball milling in step 3) are as follows: the ball milling medium is anhydrous ethanol, the weight ratio of the powder raw material, ZrO2 balls and anhydrous ethanol is 1:1.8~2.2:1.0~1.5, and the ball milling time is 20h~24h.
[0023] Preferably, the ball milling equipment used in the wet ball milling in step 3) is a planetary ball mill.
[0024] Preferably, the specific operation of the molding in step 3) is as follows: first place it in a tablet press for pre-compression, the molding pressure is 10MPa~15MPa, the holding time is 3min~5min, and then place it in a cold isostatic press for molding, the molding pressure is 270MPa~300MPa, and the holding time is 3min~5min.
[0025] Preferably, the specific operation of sintering in step 4) is as follows: first control the heating rate to be 6°C / min-8°C / min from room temperature (25°C±5°C) to 1550°C-1650°C, then keep warm for 10h-15h, and then cool to room temperature with the furnace.
[0026] Preferably, the heating furnace used for sintering in step 4) is a muffle furnace.
[0027] An aircraft engine, the environmental barrier coating on the hot end component of which comprises the above-mentioned high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion.
[0028] The beneficial effects of the present invention are as follows: the high-entropy rare earth silicate ceramic material of the present invention has excellent resistance to high-temperature CMAS corrosion (the corrosion depth after CMAS corrosion for 80 hours at 1400°C is only 75μm to 88μm, and the corrosion rate is 0.9μm / h to 1.1μm / h), and its preparation method has the advantages of simple equipment, simple and controllable process, low industrialization cost, etc. It is suitable for use in the hot end components of aerospace engines and has a very broad application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1These are XRD diagrams of the high-entropy rare earth silicate ceramic materials resistant to high-temperature CMAS corrosion according to Examples 1 to 4.
[0030] Figure 2 These are the SEM and EDS images of the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion of Example 2.
[0031] Figure 3 The BSE diagram and corrosion kinetics curve of the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion of Example 2 after being subjected to CMAS corrosion at 1400°C for 80 hours.
[0032] Figure 4 This is a BSE diagram of the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion of Example 4 after being subjected to CMAS corrosion at 1400°C for 80 hours.
[0033] Figure 5 It is the XRD diagram of the high entropy rare earth silicate ceramic material of comparative examples 1 to 3.
[0034] Figure 6 It is the BSE diagram of the high entropy rare earth silicate ceramic materials of comparative examples 1 to 3 after being corroded by CMAS at 1400°C for 80 hours. DETAILED DESCRIPTION
[0035] The present invention will be further explained and illustrated below in conjunction with specific embodiments.
[0036] The particle sizes of the Ho2O3 powder, Er2O3 powder, Yb2O3 powder and Lu2O3 powder in Examples 1 to 4 and Comparative Examples 1 to 3 are all 1 μm to 3 μm, and the purity is all ≥99.9%.
[0037] The particle size of the SiO2 powder in Examples 1 to 4 and Comparative Examples 1 to 3 is 100 nm to 200 nm, and the purity is ≥99.9%.
[0038] Embodiment 1:
[0039] A high entropy rare earth silicate ceramic material resistant to high temperature CMAS corrosion, the chemical formula of its composition is (Ho 0.1 Er 0.1 Yb 0.4 Lu 0.4 )2SiO5.
[0040] The preparation method of the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion is as follows:
[0041] 1) 3.7786 g of Ho2O3 powder, 3.8252 g of Er2O3 powder, 15.7639 g of Yb2O3 powder, 15.9175 g of Lu2O3 powder and 6.0083 g of SiO2 powder were weighed according to a molar ratio of 1:1:4:4:10 (i.e., x=0.1) and added into a planetary ball mill for wet ball milling. The process parameters of the wet ball milling are as follows: the ball milling medium is anhydrous ethanol, the weight ratio of the powder raw material, ZrO2 ball and anhydrous ethanol is 1:2:1, and the ball milling time is 6 h to obtain a mixed powder slurry;
[0042] 2) drying the mixed powder slurry in an oven, then loading it into a crucible and placing it in a muffle furnace, then heating it from room temperature to 1400° C. at a heating rate of 6° C. / min, then keeping the temperature for 2 hours, and then cooling it to room temperature with the furnace to obtain high entropy rare earth silicate ceramic powder;
[0043] 3) adding high entropy rare earth silicate ceramic powder into a planetary ball mill for wet ball milling, the process parameters of the wet ball milling are as follows: the ball milling medium is anhydrous ethanol, the weight ratio of the powder raw material, ZrO2 balls and anhydrous ethanol is 1:2:1, the ball milling time is 20 hours, and then placed in an oven for drying, and then placed in a tablet press for pre-pressing, the molding pressure is 10MPa, the pressure holding time is 3min, and then placed in a cold isostatic press for molding, the molding pressure is 270MPa, and the pressure holding time is 3min, to obtain a green body;
[0044] 4) The green body is placed in a muffle furnace, and the heating rate is controlled to be 6°C / min from room temperature to 1550°C, and then kept warm for 10 hours, and then cooled to room temperature with the furnace, thereby obtaining a high-entropy rare earth silicate ceramic material (block; denoted as Sample-1) resistant to high-temperature CMAS corrosion.
[0045] Performance Testing:
[0046] The X-ray diffraction (XRD) pattern of the high entropy rare earth silicate ceramic material (Sample-1) resistant to high temperature CMAS corrosion in this embodiment is as follows: Figure 1 shown.
[0047] Depend on Figure 1 It can be seen that the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion in this embodiment is a uniform single-phase X2-RE2SiO5, and no other impurity phases are found.
[0048] Embodiment 2:
[0049] A high entropy rare earth silicate ceramic material resistant to high temperature CMAS corrosion, the chemical formula of its composition is (Ho 0.1 Er 0.1 Yb 0.4 Lu 0.4 )2SiO5.
[0050] The preparation method of the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion is as follows:
[0051] 1) 3.7786 g of Ho2O3 powder, 3.8252 g of Er2O3 powder, 15.7639 g of Yb2O3 powder, 15.9175 g of Lu2O3 powder and 6.0083 g of SiO2 powder were weighed according to a molar ratio of 1:1:4:4:10 (i.e., x=0.1) and added into a planetary ball mill for wet ball milling. The process parameters of the wet ball milling are as follows: the ball milling medium is anhydrous ethanol, the weight ratio of the powder raw material, ZrO2 ball and anhydrous ethanol is 1:2:1.2, and the ball milling time is 8 h to obtain a mixed powder slurry;
[0052] 2) drying the mixed powder slurry in an oven, then loading it into a crucible and placing it in a muffle furnace, then heating it from room temperature to 1450° C. at a heating rate of 8° C. / min, then keeping the temperature for 3 hours, and then cooling it to room temperature with the furnace to obtain high entropy rare earth silicate ceramic powder;
[0053] 3) adding high entropy rare earth silicate ceramic powder to a planetary ball mill for wet ball milling, wherein the process parameters of the wet ball milling are as follows: the ball milling medium is anhydrous ethanol, the weight ratio of the powder raw material, ZrO2 balls and anhydrous ethanol is 1:2:1.2, the ball milling time is 22 hours, and then the powder is placed in an oven for drying, and then the powder is placed in a tablet press for pre-pressing, the molding pressure is 12 MPa, the pressure holding time is 4 minutes, and then the powder is placed in a cold isostatic press for molding, the molding pressure is 285 MPa, and the pressure holding time is 4 minutes to obtain a green body;
[0054] 4) The green body is placed in a muffle furnace, and the heating rate is controlled to be 7°C / min from room temperature to 1600°C, and then kept at this temperature for 12 hours, and then cooled to room temperature along with the furnace, thereby obtaining a high-entropy rare earth silicate ceramic material (block; denoted as Sample-2) resistant to high-temperature CMAS corrosion.
[0055] Performance Testing:
[0056] 1) The XRD pattern of the high entropy rare earth silicate ceramic material (Sample-2) resistant to high temperature CMAS corrosion in this embodiment is as follows: Figure 1 shown.
[0057] Depend on Figure 1 It can be seen that the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion in this embodiment is a uniform single-phase X2-RE2SiO5, and no other impurity phases are found.
[0058] 2) The scanning electron microscope (SEM) image and energy spectrum element distribution (EDS) image of the high entropy rare earth silicate ceramic material (Sample-2) resistant to high temperature CMAS corrosion of this embodiment are as follows: Figure 2 shown.
[0059] Depend on Figure 2 It can be seen that the average grain size of the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion in this embodiment is about 1.2 μm, and the rare earth elements are evenly distributed without obvious segregation.
[0060] 3) The high-entropy rare earth silicate ceramic material (Sample-2) resistant to high-temperature CMAS corrosion of this embodiment was tested for its high-temperature CMAS corrosion resistance. The testing process was as follows: first, CaO powder, MgO powder, Al2O3 powder and SiO2 powder were weighed according to the stoichiometric ratio of 33CaO-9MgO-13Al2O3-45SiO2 (the purity of CaO powder, MgO powder, Al2O3 powder and SiO2 powder were all analytically pure and the particle size was greater than 100 mesh), mixed and ball-milled for 6 hours, then heated to 1400°C and kept warm for 3 hours, and then cooled to obtain CMAS glass, and then the CMAS glass was ground and passed through a 100-mesh sieve to obtain CMAS powder, and then the CMAS powder was weighed and coated on the surface of the test sample, and the coating amount was 50 mg / cm 2 , and then heated to 1400℃ and kept warm for 80h to evaluate the high temperature CMAS corrosion resistance of the test sample. The corroded test sample was cut with a wire cutting machine and the corrosion depth was observed under a scanning electron microscope (the corrosion depth refers to the depth of the CMAS melt penetrating into the matrix with the uncorroded surface of the test sample as the initial interface). The backscattered scanning electron microscope (BSE) image and corrosion kinetic curve of the high entropy rare earth silicate ceramic material resistant to high temperature CMAS corrosion after CMAS corrosion for 80h at 1400℃ are shown in the figure. Figure 3 (a is a low-magnification BSE image, b is a high-magnification BSE image, and c is a corrosion kinetics curve).
[0061] Depend on Figure 3 It can be seen that the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion in this embodiment has a corrosion depth of only 75 μm after CMAS corrosion for 80 hours at 1400°C, and a corrosion rate of 0.94 μm / h. The small corrosion depth and low corrosion rate are mainly due to the formation of a very dense apatite layer and the low solubility of apatite in CMAS, which effectively blocks the further penetration of CMAS.
[0062] Embodiment 3:
[0063] A high entropy rare earth silicate ceramic material resistant to high temperature CMAS corrosion, the chemical formula of its composition is (Ho 0.1 Er 0.1 Yb 0.4 Lu 0.4 )2SiO5.
[0064] The preparation method of the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion is as follows:
[0065] 1) 3.7786 g of Ho2O3 powder, 3.8252 g of Er2O3 powder, 15.7639 g of Yb2O3 powder, 15.9175 g of Lu2O3 powder and 6.0083 g of SiO2 powder were weighed according to a molar ratio of 1:1:4:4:10 (i.e., x=0.1) and added into a planetary ball mill for wet ball milling. The process parameters of the wet ball milling are as follows: the ball milling medium is anhydrous ethanol, the weight ratio of the powder raw material, ZrO2 ball and anhydrous ethanol is 1:2:1.5, and the ball milling time is 10 h to obtain a mixed powder slurry;
[0066] 2) drying the mixed powder slurry in an oven, then loading it into a crucible and placing it in a muffle furnace, then heating it from room temperature to 1500° C. at a heating rate of 10° C. / min, then keeping the temperature for 4 hours, and then cooling it to room temperature with the furnace to obtain high entropy rare earth silicate ceramic powder;
[0067] 3) adding high entropy rare earth silicate ceramic powder to a planetary ball mill for wet ball milling, wherein the process parameters of the wet ball milling are as follows: the ball milling medium is anhydrous ethanol, the weight ratio of the powder raw material, ZrO2 balls and anhydrous ethanol is 1:2:1.5, the ball milling time is 24 hours, and then the powder is placed in an oven for drying, and then the powder is placed in a tablet press for pre-pressing, the molding pressure is 15 MPa, the pressure holding time is 5 minutes, and then the powder is placed in a cold isostatic press for molding, the molding pressure is 300 MPa, and the pressure holding time is 5 minutes to obtain a green body;
[0068] 4) The green body is placed in a muffle furnace, and the heating rate is controlled to be 8°C / min from room temperature to 1600°C, and then kept at this temperature for 15 hours, and then cooled to room temperature with the furnace, thereby obtaining a high-entropy rare earth silicate ceramic material (block; denoted as Sample-3) resistant to high-temperature CMAS corrosion.
[0069] Performance Testing:
[0070] The XRD pattern of the high entropy rare earth silicate ceramic material (Sample-3) resistant to high temperature CMAS corrosion in this embodiment is as follows: Figure 1 shown.
[0071] Depend on Figure 1 It can be seen that the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion in this embodiment is a uniform single-phase X2-RE2SiO5, and no other impurity phases are found.
[0072] Embodiment 4:
[0073] A high-entropy rare earth silicate ceramic material (block; denoted as Sample-4) resistant to high-temperature CMAS corrosion, the chemical formula of its composition is (Ho0.4 Er 0.4 Yb 0.1 Lu 0.1 )2SiO5.
[0074] The preparation of the above-mentioned high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion is exactly the same as Example 2, except that the raw materials in step 1) are adjusted to "15.1143 g of Ho2O3 powder, 15.3007 g of Er2O3 powder, 3.9410 g of Yb2O3 powder, 3.9794 g of Lu2O3 powder and 6.0083 g of SiO2 powder according to a molar ratio of 4:4:1:1:10 (i.e. x=0.4)".
[0075] Performance Test:
[0076] 1) The XRD pattern of the high entropy rare earth silicate ceramic material (Sample-4) resistant to high temperature CMAS corrosion in this embodiment is as follows: Figure 1 shown.
[0077] Depend on Figure 1 It can be seen that the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion in this embodiment is a uniform single-phase X2-RE2SiO5, and no other impurity phases are found.
[0078] 2) The BSE diagram of the high-entropy rare earth silicate ceramic material (Sample-4) resistant to high-temperature CMAS corrosion at 1400°C after CMAS corrosion for 80 hours is shown in FIG. Figure 4 shown.
[0079] Depend on Figure 4 It can be seen that the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion in this embodiment has a corrosion depth of only 88μm after CMAS corrosion for 80h at 1400°C, and a corrosion rate of 1.1μm / h. The small corrosion depth and low corrosion rate are mainly due to the generation of a very dense apatite layer, and at the same time, the solubility of apatite in CMAS is relatively small, which effectively blocks the further penetration of CMAS.
[0080] Comparative Example 1:
[0081] A high entropy rare earth silicate ceramic material (block; denoted as Sample-5), the chemical formula of its composition is (Ho 0.2 Er 0.2 Yb 0.3 Lu 0.3 )2SiO5.
[0082] The preparation of the above-mentioned high-entropy rare earth silicate ceramic material is exactly the same as Example 2, except that the raw materials in step 1) are adjusted to "7.5571 g of Ho2O3 powder, 7.6503 g of Er2O3 powder, 11.8229 g of Yb2O3 powder, 11.9381 g of Lu2O3 powder and 6.0083 g of SiO2 powder according to the molar ratio of 2:2:3:3:10 (i.e. x=0.2)".
[0083] Performance Test:
[0084] 1) The XRD pattern of the high entropy rare earth silicate ceramic material (Sample-5) of this comparative example is as follows: Figure 5 shown.
[0085] Depend on Figure 5 It can be seen that the high entropy rare earth silicate ceramic material of this comparative example is a uniform single-phase X2-RE2SiO5, and no other impurity phases are found.
[0086] 2) The BSE diagram of the high entropy rare earth silicate ceramic material (Sample-5) of this comparative example after CMAS corrosion at 1400°C for 80 hours is as follows: Figure 6 (a is a low-magnification BSE image, b is a high-magnification BSE image).
[0087] Depend on Figure 6 It can be seen that the corrosion depth of the high entropy rare earth silicate ceramic material in this comparative example after CMAS corrosion for 80 hours at 1400°C is 127μm, and the corrosion rate is 1.6μm / h. The corrosion depth and corrosion rate are significantly greater than the high entropy rare earth silicate ceramic material resistant to high temperature CMAS corrosion in Example 2. The main reason is that the density of the generated apatite layer is lower than that of Comparative Example 2.
[0088] Comparative Example 2:
[0089] A high entropy rare earth silicate ceramic material (block; denoted as Sample-6), the chemical formula of its composition is (Ho 0.25 Er 0.25 Yb 0.25 Lu 0.25 )2SiO5.
[0090] The preparation of the above-mentioned high-entropy rare earth silicate ceramic material is exactly the same as in Example 2, except that the raw materials in step 1) are adjusted to "9.4464g of Ho2O3 powder, 9.5629g of Er2O3 powder, 9.8524g of Yb2O3 powder, 9.9484g of Lu2O3 powder and 6.0083g of SiO2 powder according to the molar ratio of 2.5:2.5:2.5:2.5:10 (i.e. x=0.25)".
[0091] Performance Test:
[0092] 1) The XRD pattern of the high entropy rare earth silicate ceramic material (Sample-6) of this comparative example is as follows Figure 5 shown.
[0093] Depend on Figure 5 It can be seen that the high entropy rare earth silicate ceramic material of this comparative example is a uniform single-phase X2-RE2SiO5, and no other impurity phases are found.
[0094] 2) The BSE diagram of the high entropy rare earth silicate ceramic material (Sample-6) of this comparative example after CMAS corrosion at 1400°C for 80 hours is as follows: Figure 6 (c is a low-magnification BSE image, d is a high-magnification BSE image).
[0095] Depend on Figure 6 It can be seen that the corrosion depth of the high-entropy rare earth silicate ceramic material in this comparative example after CMAS corrosion for 80 hours at 1400°C is 178μm, and the corrosion rate is 2.2μm / h. The corrosion depth and corrosion rate are significantly greater than the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion in Example 2. The main reason is that the density of the generated apatite layer is much lower than that of Comparative Example 2, and the solubility of apatite in CMAS is also much higher than that of the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion in Example 2, which cannot effectively prevent further penetration of CMAS.
[0096] Comparative Example 3:
[0097] A high entropy rare earth silicate ceramic material (block; denoted as Sample-7), the chemical formula of its composition is (Ho 0.3 Er 0.3 Yb 0.2 Lu 0.2 )2SiO5.
[0098] The preparation of the above-mentioned high-entropy rare earth silicate ceramic material is exactly the same as Example 2, except that the raw materials in step 1) are adjusted to "11.3357 g of Ho2O3 powder, 11.4755 g of Er2O3 powder, 7.8819 g of Yb2O3 powder, 7.9587 g of Lu2O3 powder and 6.0083 g of SiO2 powder according to the molar ratio of 3:3:2:2:10 (i.e. x=0.3)".
[0099] Performance Test:
[0100] 1) The XRD pattern of the high entropy rare earth silicate ceramic material (Sample-7) of this comparative example is as follows: Figure 5 shown.
[0101] Depend on Figure 5It can be seen that the high entropy rare earth silicate ceramic material of this comparative example is a uniform single-phase X2-RE2SiO5, and no other impurity phases are found.
[0102] 2) The BSE graph of the high entropy rare earth silicate ceramic material (Sample-7) of this comparative example after CMAS corrosion at 1400°C for 80 hours is as follows: Figure 6 (e is a low-magnification BSE image, f is a high-magnification BSE image).
[0103] Depend on Figure 6 It can be seen that the corrosion depth of the high-entropy rare earth silicate ceramic material in this comparative example after CMAS corrosion for 80 hours at 1400°C is 165μm, and the corrosion rate is 2.1μm / h. The corrosion depth and corrosion rate are significantly greater than the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion in Example 2. The main reason is that the density of the generated apatite layer is much lower than that of Comparative Example 2, and the solubility of apatite in CMAS is also much higher than that of the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion in Example 2, which cannot effectively prevent further penetration of CMAS.
[0104] Combining Examples 1 to 4 and Comparative Examples 1 to 3, it can be found that the chemical formula of the components of the high entropy rare earth silicate ceramic material (Ho x Er x Yb 0.5-x Lu 0.5-x )2SiO5, when x=0.05-0.15 or 0.35-0.45, the high-entropy rare earth silicate ceramic material has excellent resistance to high-temperature CMAS corrosion. This shows that the ratio between the rare earth elements has a great influence on the resistance to high-temperature CMAS corrosion. The main reason lies in the synergistic effect between the rare earth elements.
[0105] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A high entropy rare earth silicate ceramic material resistant to high temperature CMAS corrosion, characterized in that: The chemical formula of the components is (Ho x Er x Yb 0.5-x Lu 0.5-x )2SiO5, wherein x=0.05~0.15 or 0.35~0.
45.
2. The high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion according to claim 1, characterized in that: The high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion has a corrosion depth of 75 μm to 88 μm and a corrosion rate of 0.9 μm / h to 1.1 μm / h after CMAS corrosion for 80 hours at 1400°C.
3. A method for preparing a high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion as claimed in claim 1 or 2, characterized in that: The following steps are involved: 1) Ho2O3 powder, Er2O3 powder, Yb2O3 powder, Lu2O3 powder and SiO2 powder are weighed according to the stoichiometric ratio, mixed and wet-milled to obtain a mixed powder slurry; 2) drying the mixed powder slurry and then calcining it to obtain high entropy rare earth silicate ceramic powder; 3) wet-milling and drying the high-entropy rare earth silicate ceramic powder and then forming it to obtain a green body; 4) Sintering the green body to obtain a high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion.
4. The preparation method according to claim 3, characterized in that: The particle size of the Ho2O3 powder in step 1) is 1μm~3μm, and the purity is ≥99.9%; the particle size of the Er2O3 powder in step 1) is 1μm~3μm, and the purity is ≥99.9%; the particle size of the Yb2O3 powder in step 1) is 1μm~3μm, and the purity is ≥99.9%; the particle size of the Lu2O3 powder in step 1) is 1μm~3μm, and the purity is ≥99.9%; the particle size of the SiO2 powder in step 1) is 100nm~200nm, and the purity is ≥99.9%.
5. The preparation method according to claim 3 or 4, characterized in that: Step 1) The process parameters of the wet ball milling are as follows: the ball milling medium is anhydrous ethanol, the weight ratio of the powder raw material, ZrO2 balls and anhydrous ethanol is 1:1.8~2.2:1.0~1.5, and the ball milling time is 6h~10h.
6. The preparation method according to claim 3, characterized in that: Step 2) The specific operation of the calcination is as follows: first control the heating rate to be 6°C / min-10°C / min from room temperature to 1400°C-1500°C, then keep the temperature for 2h-4h, and then cool to room temperature with the furnace.
7. The preparation method according to claim 3, characterized in that: Step 3) The process parameters of the wet ball milling are as follows: the ball milling medium is anhydrous ethanol, the weight ratio of the powder raw material, ZrO2 balls and anhydrous ethanol is 1:1.8~2.2:1.0~1.5, and the ball milling time is 20h~24h.
8. The preparation method according to claim 3 or 7, characterized in that: The specific operation of the molding in step 3) is as follows: firstly, the tablet is placed in a tablet press for pre-compression, the molding pressure is 10MPa-15MPa, the pressure holding time is 3min-5min, and then, the tablet is placed in a cold isostatic press for molding, the molding pressure is 270MPa-300MPa, and the pressure holding time is 3min-5min.
9. The preparation method according to claim 3, characterized in that: Step 4) The specific operation of the sintering is as follows: first control the heating rate to be 6°C / min-8°C / min from room temperature to 1550°C-1650°C, then keep the temperature for 10h-15h, and then cool to room temperature with the furnace.
10. An aircraft engine, characterized in that: The environmental barrier coating on the hot end component comprises the high-entropy rare earth silicate ceramic material resistant to high-temperature CMAS corrosion as claimed in claim 1 or 2.
Citation Information
Patent Citations
Light and heavy rare earth mixed high-entropy rare earth silicate compact block and preparation method thereof
CN113024232A
High-entropy rare earth silicate ceramic powder as well as preparation method and application thereof
CN117142854A
High-entropy rare earth silicate ceramic coating material and preparation method thereof
CN117383919A
High-entropy rare earth titanate ceramic coating material and preparation method thereof
CN117383926A
High-entropy rare earth monosilicate environmental barrier coating as well as preparation method and application thereof
CN117550883A
Cited By
Si-site-doped rare earth monosilicate ceramic as well as preparation method and application thereof
CN121248289A
A medium-entropy rare earth pyrosilicate coating material, a step-by-step hot pressing preparation method thereof and application thereof
CN122831734A