Nitrogen-containing heterocyclic resin as well as preparation method and application thereof
Through the design and synthesis of nitrogen-containing heterocyclic resins, the problem of insufficient selectivity of existing resin solid-phase extraction methods in adsorbing metals such as nickel, copper, and cobalt has been solved, and high selective adsorption and excellent separation effects have been achieved, especially in It has advantages in the acidic environment for impurity ion separation of copper, nickel and cobalt.
Patent Information
- Application Number
- CN202310532657.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-12
AI Technical Summary
The existing resin solid-phase extraction methods are insufficient in adsorbing metals such as nickel, copper, cobalt, etc., and it is difficult to meet the high selectivity needs.
A resin material with high selective adsorption effect is prepared by reacting the resin matrix with a connecting bridge and specific substitution of the nitrogen-containing heterocyclic substituent, and synthesized in an alkaline solution to improve the synthesis efficiency.
High selective adsorption of metals such as nickel, copper, and cobalt is achieved, the metal separation effect is improved, and excellent separation ability is shown in acidic solutions, especially the impurity ion separation of copper, nickel, and cobalt.
Smart Images

Figure CN118930696A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of organic compound preparation, and in particular to a nitrogen-containing heterocyclic resin and a preparation method and application thereof. Background Art
[0002] Resin solid phase extraction is an important method in metal purification and separation processes. It has a wide range of applications in metal separation and purification, including chemical industry, electroplating, metallurgy, non-ferrous metal mining, and new energy industries. Resin solid phase extraction can make the atoms on the functional groups on the resin react with the metal through material design to form a chelate with a stable structure, thereby selectively separating and enriching the metal elements in the dilute solution. Compared with the traditional solvent extraction method, the resin method has the characteristics of fast phase separation, simple operation, low pollution, and low process cost.
[0003] However, the existing resin solid phase extraction method still cannot meet the requirements of high selective adsorption, especially in the application of adsorbing metals such as nickel, copper, cobalt, etc.
[0004] Therefore, it is necessary to provide a new resin material and a method for solid phase extraction of metals to further improve the selectivity in metal adsorption, thereby improving the separation effect of metal elements, especially metals such as nickel, copper, and cobalt. Summary of the invention
[0005] In view of this, the present invention provides a resin material having a better selective adsorption effect on metal elements, and a preparation method and use thereof.
[0006] As described above, the present invention provides the following technical solutions:
[0007] In a first aspect, the present invention discloses a nitrogen-containing heterocyclic resin, comprising a nitrogen-containing heterocyclic resin represented by the following structural formula (1):
[0008]
[0009] in:
[0010] P is the resin matrix;
[0011] n and m represent any integer from 2 to 6 respectively;
[0012] R1, R2, R3 and R4, which are the same or different, are nitrogen-containing heterocyclic substituents.
[0013] For the purpose of the present invention, the resin matrix P is not particularly limited.
[0014] Preferably, the resin matrix P is selected from any one or more of polystyrene resin, copolymer of styrene and divinylbenzene, phenolic resin polymer, polyacrylic resin, and silicon-based resin.
[0015] According to the above structural formula (1), wherein n and m can be any integer from 2 to 10, preferably, n and m are selected from any integer from 2 to 6, wherein the connecting bridge -CH2-N-(CH2) n -N- or -CH2-N-(CH2) m -N- can be
[0016] -CH2-N-(CH2)2-N-;
[0017] -CH2-N-(CH2)3-N-;
[0018] -CH2-N-(CH2)4-N-;
[0019] -CH2-N-(CH2)5-N-. Nitrogen-containing heterocyclic resins containing these connecting bridges have better selective adsorption effects.
[0020] Further, according to the present invention, the nitrogen-containing heterocyclic substituents R1, R2, R3 and R4 are independently pyridine groups, imidazole groups, benzimidazole groups, pyrazole groups, quinoline groups, pyrazine groups, triazine groups or triazole groups. In other words, what groups R1, R2, R3 and R4 are each is not affected by other nitrogen-containing heterocyclic substituents.
[0021] Furthermore, the nitrogen-containing heterocyclic substituents R1, R2, R3 and R4 are independently selected from any of the following groups:
[0022]
[0023]
[0024] The above groups have a good effect of selectively adsorbing metals.
[0025] Furthermore, the nitrogen-containing heterocyclic substituents R1, R2, R3 and R4 are independently selected from any of the following groups:
[0026]
[0027]
[0028] The above groups are preferred because of their better metal adsorption effect.
[0029] In a second aspect, the present invention provides a method for preparing a nitrogen-containing heterocyclic resin, which is used to prepare the nitrogen-containing heterocyclic resin having the above structural formula (1) in the first aspect, and the method comprises the following steps:
[0030] S10: providing a resin base material, wherein the resin base material is a resin containing primary amino groups;
[0031] S20: The primary amino group of the resin base material is reacted with X(CH2) m Y undergoes a substitution reaction to obtain a first intermediate compound, wherein:
[0032] X and Y are independently chlorine, bromine or iodine;
[0033] m is any integer from 2 to 6;
[0034] S30: making the first intermediate compound and R a NHR b Further substitution reaction occurs to obtain the nitrogen-containing heterocyclic resin, wherein R a and R b are independently selected from R1, R2, R3 and R4. That is, the compound R that undergoes substitution reaction with the first intermediate compound to generate the nitrogen-containing heterocyclic resin of formula (1) a NHR b , can be any one or more of R1NHR1, R1NHR3, R1NHR4, R3NHR2, R4NHR2, R3NHR4, etc., as long as the corresponding selection is made according to the target compound. Among them, R1, R2, R3 and R4 are as described above, and will not be repeated.
[0035] Furthermore, the resin base material is selected from any one or more of polystyrene microspheres containing primary amino groups, modified phenolic resins containing primary amino groups, polyacrylic acid resins containing primary amino groups, and silicon-based resins containing primary amino groups.
[0036] Furthermore, the resin base material and X(CH2) m Y and R a NHR b The molar ratio is 1:(0.5-4):(0.5-4).
[0037] Furthermore, the reaction conditions of the substitution reaction in step S20 and step S30 are the same, both of which are carried out in an alkaline solution under heating conditions. In an alkaline solution under heating conditions, it is beneficial to promote the substitution reaction and improve the synthesis efficiency and yield.
[0038] Furthermore, the base contained in the alkaline solution is the X(CH2) m Y or R a NHR b 1-3 times the equivalent.
[0039] Further, the solvent of the alkaline solution is the X(CH2) m Y or Ra NHR b The mass of the raw material is 2-50 times of that of the raw material, the heating temperature is 40-120°C, and the reaction time is 3-36 hours.
[0040] Furthermore, the base is selected from any one or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium carbonate, potassium bicarbonate, potassium hydroxide, triethylamine, and N,N-diisopropylethylamine. These bases are easy to obtain, low in price, easy to recycle, safe and stable, and are therefore preferred.
[0041] Furthermore, the solvent is selected from any one or more of water, N,N-dimethylformamide, dimethyl sulfoxide, toluene, tetrahydrofuran, ethanol, acetonitrile, and acetone.
[0042] In a third aspect, there is provided a use of the nitrogen-containing heterocyclic resin of the first aspect for adsorbing metals, wherein the metal is any one or more of mercury, gallium, iron, cobalt, nickel, copper, zinc, lead, indium, cadmium, manganese, aluminum, uranium, vanadium, platinum group elements, gold, and silver.
[0043] Furthermore, the metal comprises one or more of cobalt, nickel, copper, zinc, cadmium, manganese and aluminum; preferably comprises one or more of nickel, copper and cobalt.
[0044] Further, it is used for adsorption of said metals in hydrometallurgy, waste disposal, recycling industry or electroplating.
[0045] In a fourth aspect, an adsorbent for solid phase extraction of metal elements is provided, which comprises the nitrogen-containing heterocyclic resin of the first aspect. Of course, as an adsorbent, in addition to the nitrogen-containing heterocyclic resin, other materials may also be contained according to specific use requirements. For example, in addition to adsorbing metal elements, if it is also desired to adsorb specific organic compounds at the same time, the adsorbent may also contain materials for adsorbing specific organic compounds.
[0046] In a fifth aspect, a method for solid phase extraction of metal elements is provided, which utilizes the adsorbent provided in the fourth aspect.
[0047] Specifically, the method for solid phase extraction of metal elements may include the following steps: using an adsorbent containing a nitrogen-containing heterocyclic resin to extract the metal in a metal-containing solution to obtain a metal-loaded nitrogen-containing heterocyclic resin and a residual water phase; then washing and stripping the metal-loaded nitrogen-containing heterocyclic resin in sequence to obtain a metal-rich stripping solution and a stripped resin.
[0048] The metal adsorbed by the solid phase extraction method of metal elements is selected from any one or more of mercury, gallium, iron, cobalt, nickel, copper, zinc, lead, indium, cadmium, manganese, aluminum, uranium, vanadium, platinum group elements, gold and silver.
[0049] Preferably, the adsorbed metal is selected from one or more of cobalt, nickel, copper, zinc, cadmium, manganese and aluminum, and further selected from one or more of nickel, copper and cobalt.
[0050] Preferably, the detergent used for washing in the method is a dilute acid solution, and the stripping agent used for stripping is a sulfuric acid or hydrochloric acid solution, further a sulfuric acid solution.
[0051] The method is simple to operate and has good metal separation effect.
[0052] The above technical solution of the present invention has at least one of the following beneficial effects:
[0053] The nitrogen-containing heterocyclic resin according to the embodiment of the present invention has high selectivity and loading capacity for metal ions through the nitrogen-containing functional group, thus providing a new separation material for extraction process technology;
[0054] Moreover, the selectivity for metal ions can be further improved by increasing the number of nitrogen-containing functional groups and amine nitrogen;
[0055] In addition, the nitrogen-containing heterocyclic resin of the present invention can adsorb copper, nickel, cobalt, etc. in an acidic solution (pH <3), and can achieve effective separation of copper, nickel, and cobalt, especially copper and iron impurity ions;
[0056] In addition, the preparation method provided by the present invention has simple process. DETAILED DESCRIPTION
[0057] In the following, various aspects of the invention will be described in more detail as well as further objects, features and advantages.
[0058] Unless otherwise defined, the technical terms or scientific terms used in the present invention shall have the common meanings understood by persons with ordinary skills in the field to which the present invention belongs. The words "first", "second" and similar words used in the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components.
[0059] Hereinafter, the nitrogen-containing heterocyclic resin according to the present invention is first described.
[0060] The nitrogen-containing heterocyclic resin according to the present invention comprises a nitrogen-containing heterocyclic resin represented by the following structural formula (1):
[0061]
[0062] in:
[0063] P is the resin matrix;
[0064] -CH2-N-(CH2) n -N- or -CH2-N-(CH2)m -N- is a connecting bridge between P and R1, R2, R3 or R4;
[0065] n and m represent any integer from 2 to 6;
[0066] R1, R2, R3 and R4, which are the same or different, are nitrogen-containing heterocyclic substituents.
[0067] The inventors unexpectedly found that the nitrogen-containing heterocyclic resin according to the present invention has high selectivity for metal ions and, on this basis, also has a higher loading capacity; and, by increasing the number of nitrogen-containing functional groups, the selectivity for metal ions can be further improved; in addition, the nitrogen-containing heterocyclic resin of the present invention can adsorb copper, nickel, etc. in an acidic solution (pH<3), providing a new separation material for new extraction process technology.
[0068] Further, according to the above structural formula (1), n and m can be any integer from 2 to 10, preferably n and m are any integer from 2 to 6; wherein the connecting bridge -CH2-N-(CH2) n -N- or -CH2-N-(CH2) m -N- can be
[0069] -CH2-N-(CH2)2-N-;
[0070] -CH2-N-(CH2)3-N-;
[0071] -CH2-N-(CH2)4-N-;
[0072] -CH2-N-(CH2)5-N-.
[0073] Preferably, the structural formula of the connecting bridge is -CH2-N-(CH2)2-N-.
[0074] Furthermore, the resin matrix P is not particularly limited, and is preferably selected from any one or more of polystyrene resin, copolymer of styrene and divinylbenzene, phenolic resin polymer, polyacrylic resin, and silicon-based resin.
[0075] Preferably, the resin matrix P described in the present invention is one or more of polystyrene resin and copolymers of styrene and divinylbenzene.
[0076] Further, the nitrogen-containing heterocyclic substituents R1, R2, R3 and R4 of the present invention are independently pyridine groups, imidazole groups, benzimidazole groups, pyrazole groups, quinoline groups, pyrazine groups, triazine groups or triazole groups. The so-called pyridine groups include pyridyl and its derivatives, and the like. These nitrogen-containing functional groups have high selectivity for metal ions and are therefore preferred.
[0077] The R1, R2, R3 and R4 are the same or different groups, and further, are the same group.
[0078] Furthermore, the nitrogen-containing heterocyclic substituents R1, R2, R3 and R4 are independently selected from any of the following groups:
[0079]
[0080]
[0081] These nitrogen-containing functional groups are preferred because they have strong selectivity for metals.
[0082] Furthermore, the nitrogen-containing heterocyclic substituents R1, R2, R3 and R4 are independently selected from any of the following groups:
[0083]
[0084]
[0085] The present invention provides a nitrogen-containing heterocyclic resin selected from the following structures:
[0086]
[0087]
[0088] Next, the method for preparing the nitrogen-containing heterocyclic resin represented by the structural formula (1) is described.
[0089] The nitrogen-containing heterocyclic resin represented by the above structural formula (1) has higher selectivity for metal ions.
[0090] The nitrogen-containing heterocyclic resin represented by the above structural formula (1) is prepared using a resin containing primary amino groups as a starting material.
[0091] The following is a further explanation of the exemplary preparation method.
[0092] The method according to the present invention comprises the following steps:
[0093] S10: providing a resin base material, wherein the resin base material is a resin containing primary amino groups;
[0094] S20: The primary amino group of the resin base material is reacted with X(CH2) m Y undergoes a substitution reaction to obtain a first intermediate compound, wherein:
[0095] X and Y are independently chlorine, bromine or iodine, and m is any integer from 2 to 6;
[0096] S30: making the first intermediate compound and Ra NHR b Further substitution reaction occurs to obtain the nitrogen-containing heterocyclic resin, wherein R a and R b They are independently selected from R1, R2, R3 and R4. R1, R2, R3 and R4 are as described above, and their detailed description is omitted here.
[0097] Specifically, the synthetic route of the method of the present invention is shown in the following formula:
[0098]
[0099] Wherein, preferably, the resin base material is selected from any one or more of polystyrene microspheres containing primary amino groups, modified phenolic resins containing primary amino groups, polyacrylic acid resins containing primary amino groups, and silicon-based resins containing primary amino groups.
[0100] Preferably, the resin base material and X(CH2) m Y and R a NHR b The molar ratio is 1:(0.5-4):(0.5-4). Further, it is 1:(1-3):(1-3).
[0101] Preferably, the reaction conditions of the substitution reaction in step S20 and step S30 are the same, and both are carried out in an alkaline solution under heating conditions.
[0102] Preferably, the base contained in the alkaline solution is the X(CH2) m Y or R a NHR b 1-3 times the equivalent.
[0103] Preferably, the solvent of the alkaline solution is the X(CH2) m Y or R a NHR b The mass of the raw material is 2-50 times of that of the raw material, the heating temperature is 40-120°C, and the reaction time is 3-36 hours.
[0104] Preferably, the base is selected from any one or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium carbonate, potassium bicarbonate, potassium hydroxide, triethylamine, and N,N-diisopropylethylamine.
[0105] Preferably, the solvent is selected from any one or more of water, N,N-dimethylformamide, dimethyl sulfoxide, toluene, tetrahydrofuran, ethanol, acetonitrile and acetone.
[0106] Of course, the alkali used in step S30 and step S20 and the amount used may be different from step S20 as long as they are within the above ranges.
[0107] It should be noted that, similarly, in the above method, there is also R a and R b In the case of the same nitrogen-containing heterocyclic substituent and different nitrogen-containing heterocyclic substituents, as long as the corresponding composition of R a NHR b Then, select R a NHR a or R a NHR b That's it.
[0108] The "selectivity" described in the present invention is represented by the separation coefficient β of the metal element. Further, the separation coefficient is obtained by the following formula:
[0109] β A / B =D A / D B =E A .(1-E B ) / ((1-E A ).E B )
[0110] Where D A It indicates the ratio of the content of metal element A in the resin to the content of metal element A in the raffinate water phase after one extraction is completed;
[0111] D B It indicates the ratio of the content of metal element B in the resin to the content of metal element B in the raffinate water phase after one extraction is completed;
[0112] E A 、E B It represents the extraction rate of metal element A and metal element B (extraction rate E=the content of metal element in the resin after one extraction / the content of metal element in the initial water phase×100%).
[0113] The metal extraction rate in the formula is measured by the following method:
[0114] Resin pretreatment: Mix the resin with 2 mol / L sulfuric acid and stir until the supernatant is colorless, then wash with 0.25 mol / L sodium hydroxide solution until the supernatant is alkaline, then wash the resin with pure water until it is neutral, filter and set aside;
[0115] 30 mL of sulfate solution containing 0.05 g / L of each metal element was prepared as the initial aqueous phase, and the pH value of the initial aqueous phase was adjusted. Then, it was mixed and stirred with 5 g of pretreated resin at room temperature for 60 min at a rotation speed of 250 rpm / min to allow the adsorption to reach equilibrium. After stirring, the solid-liquid separation was performed to obtain a raffinate (equilibrium) aqueous phase, and the concentration of each metal element in the raffinate aqueous phase was determined by inductively coupled plasma emission spectroscopy (ICP), and the content of the metal elements in the resin was calculated by subtraction.
[0116] The "load amount" described in the present invention is obtained by the following method:
[0117] Prepare 0.5 mol / L sulfate solution of each metal element respectively, adjust the pH value of the initial aqueous phase, take 2 g of the pretreated resin in a beaker respectively, add 20 mL of the prepared metal element solution to each, stir at room temperature for 60 min, rotate at 250 rpm / min, after stirring, separate the solid and liquid, and obtain the raffinate aqueous phase. Repeat three times, contacting with a fresh initial aqueous phase each time, and use inductively coupled plasma emission spectroscopy (ICP) to determine the concentration of each metal element in the raffinate aqueous phase. The content of the metal element in the resin is calculated by subtraction to obtain the loading capacity of the resin for each metal element.
[0118] Example
[0119] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described in conjunction with the embodiments below. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the described embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0120] Example 1: Preparation of Resin 1
[0121] The synthetic route of resin 1 is as follows:
[0122]
[0123] Take 10g (30mmol, -NH2) of primary amino polystyrene microspheres (Lanxiao Technology, model LX-D30) and 11.34g (72mmol) of 1-bromo-3-chloropropane in a 100ml three-necked flask, add 60g of N,N-dimethylformamide and 7.27g (72mmol) of triethylamine in sequence, heat to 60℃ under mechanical stirring, react for 18 hours, and the reaction generates Microspheres (hereinafter referred to as intermediate microspheres).
[0124] The intermediate microspheres were filtered out by suction, rinsed twice with N,N-dimethylformamide, placed in a 100 ml three-necked flask, and 14.35 g (72 mmol) of dimethylpyridinamine, 60 g of N,N-dimethylformamide, and 7.63 g (72 mmol) of sodium carbonate were added to the reaction system in sequence. The reaction was carried out at 80° C. for 24 hours to obtain resin 1. The yield of resin 1 was 80%.
[0125] Example 2: Preparation of Resin 2
[0126] The synthetic route of resin 2 is as follows:
[0127]
[0128] Take 10g (30mmol, -NH2) of primary amino polystyrene microspheres (Lanxiao Technology, model LX-D30) and 11.34g (72mmol) of 1-bromo-3-chloropropane in a 100ml three-necked flask, add 100g of ethanol and 2.88g (72mmol) of sodium hydroxide in turn, heat to 60℃ under mechanical stirring, react for 24 hours, and the reaction generates Microspheres (hereinafter referred to as intermediate microspheres).
[0129] The intermediate microspheres were filtered out by suction, and washed twice with dichloroethane, three times with ethanol, and three times with water. The intermediate microspheres were placed in a 100 ml three-necked flask, and 16.37 g (72 mmol) of bis[(6-methylpyridin-2-yl)methyl]amine, 100 g of ethanol, and 7.63 g (72 mmol) of sodium carbonate were added to the reaction system in sequence. The reaction was carried out at 60° C. for 24 hours to obtain resin 2, and the yield of resin 2 was 78%.
[0130] Example 3: Preparation of Resin 3
[0131] The synthetic route of resin 3 is as follows:
[0132]
[0133] Take 10g (30mmol, -NH2) of primary amino polystyrene microspheres (Lanxiao Technology, model LX-D30) and 10.33g (72mmol) of 1-bromo-2-chloroethane in a 100ml three-necked flask, add 60g of acetone and 7.27g (72mmol) of triethylamine in sequence, heat to 60℃ under mechanical stirring, react for 24 hours, and the reaction generates Microspheres (hereinafter referred to as intermediate microspheres).
[0134] The intermediate microspheres were filtered out by suction, rinsed twice with acetone, placed in a 100 ml three-necked flask, and added into the reaction system in sequence: 14.4 g (72 mmol), 60 g acetone, 7.63 g (72 mmol) of sodium carbonate were reacted at 80°C for 18 hours to obtain resin 3 with a yield of 83%.
[0135] Performance Evaluation
[0136] Evaluation Experiment 1 (Evaluation of the Performance of Resin 1 Obtained in Example 1)
[0137] Configuration containing Cu 2+ 、Ni 2+ 、Co 2+ 、Al 3+ , Fe 3+ , Mn 2+ 、Cd 2+ 、Zn 2+ , Ca 2+ Mg 2+ Cr 2+ , Li + 30 mL of each 0.05 g / L sulfate solution was used as the initial aqueous phase, and the pH value of the initial aqueous phase was adjusted to 1. Then, 5 g of pretreated resin 1 was mixed and stirred at room temperature for 60 min, with a rotation speed of 250 rpm / min, so that the adsorption reached equilibrium. After the extraction was completed, the concentration of each metal ion in the raffinate aqueous phase was determined by inductively coupled plasma emission spectroscopy (ICP), and the content of metal ions in the resin was determined by subtraction. The extraction rate of resin 1 for each ion was calculated, and then the separation coefficient between resin 1 and each ion was calculated based on the extraction rate (Table 1).
[0138] Table 1 Separation coefficients of resin 1 for various ions when the initial aqueous phase pH is about 1
[0139]
[0140]
[0141] The results show that when the pH value of the initial aqueous phase is about 0.5, the extraction rates of Cu, Ni and Co by resin 1 are 99.9%, 56.1% and 36.7%, respectively, the extraction rate of Fe is 5.6%, and the extraction rates of other metals are less than 5%; when the pH value of the initial aqueous phase is about 1, the extraction rates of Cu, Ni and Co by resin 1 are 99.8%, 90.7% and 85.9%, respectively, the extraction rates of Zn, Cd and Fe are 62.6%, 66.5% and 30.2%, respectively, and the extraction rates of other metals are less than 12%; when the pH value of the initial aqueous phase is about 2.5, the extraction rates of Ni, Co, Cu, Fe, Mn, Cd, Zn, Al and Cr by resin 1 are all greater than 95%, and the extraction rates of Ca, Mg and Li are all less than 10%.
[0142] As shown in Table 1, when the initial pH value of the aqueous phase is about 1, the separation coefficients of Cu and Ni, Co, Zn, Cd, and Fe are 51.1, 82.1, 298, 251, and 1153, respectively, and the separation coefficients with other metal ions are all above 4000. The separation coefficients of Ni and Co, Zn, Cd, and Fe are 1.6, 5.8, 4.9, and 22.6, respectively, and the separation coefficients of Co and Zn, Cd, and Fe are 3.6, 3.1, and 14.1, respectively. This shows that copper, nickel, and cobalt (especially copper) have a high degree of separation from impurity ions such as iron. The above results show that the resin has good selectivity for copper, nickel, and cobalt (especially copper).
[0143] Evaluation experiment 2 (performance comparison between resin 1 and commercially available resin Dowex M4195)
[0144] The method in the above-mentioned evaluation experiment 1 was referred to, except that the resin 1 was replaced with Dowex M4195 (commercially available from Dow). The results are shown in Table 2.
[0145] Table 2 Separation coefficients of resin 1 and Dowex M4195 for various ions
[0146]
[0147]
[0148] As shown in Table 2, under the same experimental conditions, compared with Dowex M4195, the separation coefficient of resin 1 for each ion is higher, about 1.5 times higher. When the initial aqueous phase pH value is about 1, the separation coefficients of resin 1 for Cu / Fe, Cu / Zn, Cu / Cd, Ni / Fe, and Co / Fe are 1153, 298, 251, 22.6, and 14.1, respectively, while the separation coefficients of Dowex M4195 for Cu / Fe, Cu / Zn, Cu / Cd, Ni / Fe, and Co / Fe are 72.1, 62.1, 74.6, 8.9, and 4.8, respectively. The results show that compared with Dowex M4195, resin 1 has significant selectivity for copper, nickel, and cobalt (especially copper).
[0149] Evaluation Experiment 3 (Evaluation of the Performance of Resin 2 Obtained in Example 2)
[0150] Referring to the method in the above-mentioned evaluation experiment 1, the difference from the evaluation experiment 1 is that resin 1 is replaced by resin 2. The results show that when the pH value of the initial aqueous phase is about 1, the extraction rates of resin 2 for Cu, Ni and Co are 99.9%, 92.7% and 89.2%, respectively, the extraction rates for Zn, Cd and Fe are 66.6%, 70.0% and 38.0%, respectively, and the extraction rates for other metals are all less than 10%. At this pH, the separation coefficients of Cu and Ni, Co, Zn, Cd and Fe are 78.5, 121, 650, 539 and 1632, respectively, and the separation coefficients with other metal ions are all above 9000, the separation coefficients of Ni and Co, Zn, Cd and Fe are 1.5, 8.3, 6.9 and 20.8, respectively, and the separation coefficients of Co and Zn, Cd and Fe are 4.2, 3.6 and 13.5, respectively. This shows that copper, nickel and cobalt (especially copper) have a high degree of separation from impurity ions such as iron. The above results show that compared with Dowex M4195, resin 2 has significant selectivity for copper, nickel and cobalt (especially copper).
[0151] Evaluation Experiment 4 (Evaluation of the Performance of Resin 3 Obtained in Example 3)
[0152] Referring to the method in the above-mentioned evaluation experiment 1, the difference from the evaluation experiment 1 is that resin 1 is replaced by resin 3, and the initial pH value of the aqueous phase is adjusted to 1.2. The results show that when the pH value of the initial aqueous phase is about 1.2, the extraction rates of resin 3 for Cu, Ni and Co are 99.2%, 91.0% and 71.6%, respectively, the extraction rates for Zn, Cd and Fe are 47.3%, 54.6% and 27.9%, respectively, and the extraction rates for other metals are less than 15%. At this pH, the separation coefficients of Cu with Ni, Co, Zn, Cd and Fe are 12.2, 49.1, 138, 103 and 321, respectively, and the separation coefficients with other metal ions are all above 800, the separation coefficients of Ni with Co, Zn, Cd and Fe are 4.0, 11.3, 8.4 and 26.2, respectively, and the separation coefficients of Co with Zn, Cd and Fe are 2.8, 2.1 and 6.5. This shows that copper, nickel, and cobalt (especially copper) have a high degree of separation from impurity ions such as iron.
[0153] Evaluation Experiment 5 (Performance Comparison between Resin 3 and Commercially Available Resin Dowex M4195)
[0154] The method in Evaluation Experiment 4 was referred to, except that Resin 3 was replaced with Dowex M4195 (commercially available from Dow). The results are shown in Table 3.
[0155] Table 3 Separation coefficients of resin 3 and Dowex4195 for various ions
[0156]
[0157] As shown in Table 3, under the same experimental conditions, compared with Dowex M4195, the separation coefficient of resin 3 for each ion is higher, about 1 times higher. When the initial aqueous phase pH value is about 1.2, the separation coefficients of resin 3 for Cu / Fe, Cu / Zn, Cu / Cd, Ni / Fe, and Co / Fe are 321, 138, 103, 26.2, and 6.5, respectively, while the separation coefficients of Dowex M4195 for Cu / Fe, Cu / Zn, Cu / Cd, Ni / Fe, and Co / Fe are 48.8, 40.1, 47.3, 8.4, and 1.8, respectively. Compared with Dowex M4195, resin 3 has significant selectivity for copper, nickel, and cobalt (especially copper).
[0158] Evaluation experiment 6
[0159] The results of the load capacity test on the products in Examples 1 to 3 are shown in Table 4.
[0160] Table 4 Initial aqueous phase pH value is 1.2, extraction is performed 3 times, and the loading amount of copper and nickel on the resin / mg / g
[0161] Resin copper nickel Resin 1 88 58 Resin 2 90 60 Resin 3 85 57
[0162] It can be seen from Table 4 that the copper and nickel loadings of resin 1, resin 2, and resin 3 are high. When the initial aqueous phase pH value is 1.2, the extraction is repeated three times, and each time the initial aqueous phase is contacted, the copper loadings of resin 1, resin 2, and resin 3 are 88 mg / g, 90 mg / g, and 85 mg / g, respectively, and the nickel loadings are 58 mg / g, 60 mg / g, and 57 mg / g, respectively.
[0163] Evaluation experiment 7
[0164] Repeatability test
[0165] The resin products of Examples 1 to 3 were extracted and regenerated 6 times, and the loading amounts of Cu and Ni of the resin products of Examples 1 to 3 were not much different from those of the first time.
[0166] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and changes can be made without departing from the principles of the present invention. These improvements and changes should also be regarded as the scope of protection of the present invention.
Claims
1. A nitrogen-containing heterocyclic resin, characterized in that The invention comprises a nitrogen-containing heterocyclic resin represented by the following structural formula (1): in: P is the resin matrix; n and m represent any integer from 2 to 6 respectively; R1, R2, R3 and R4, which are the same or different, are nitrogen-containing heterocyclic substituents.
2. The nitrogen-containing heterocyclic resin according to claim 1, characterized in that The resin matrix P is selected from any one or more of polystyrene resin, copolymer of styrene and divinylbenzene, phenolic resin polymer, polyacrylic resin, and silicon-based resin.
3. The nitrogen-containing heterocyclic resin according to claim 1, characterized in that The nitrogen-containing heterocyclic substituents R1, R2, R3 and R4 are independently pyridine groups, imidazole groups, benzimidazole groups, pyrazole groups, quinoline groups, pyrazine groups, triazine groups or triazole groups.
4. The nitrogen-containing heterocyclic resin according to claim 3, characterized in that The nitrogen-containing heterocyclic substituents R1, R2, R3 and R4 are independently selected from any of the following groups:
5. A method for preparing the nitrogen-containing heterocyclic resin according to any one of claims 1 to 4, characterized in that: The steps include: S10: providing a resin base material, wherein the resin base material is a resin containing primary amino groups; S20: The primary amino group of the resin base material is reacted with X(CH2) m Y undergoes a substitution reaction to obtain a first intermediate compound, wherein: X and Y are independently chlorine, bromine or iodine; m is any integer from 2 to 6; S30: making the first intermediate compound and R a NHR b Further substitution reaction occurs to obtain the nitrogen-containing heterocyclic resin, wherein R a and R b are independently selected from R1, R2, R3 and R4.
6. The preparation method according to claim 5, characterized in that: The resin base material is selected from any one or more of polystyrene microspheres containing primary amino groups, modified phenolic resins containing primary amino groups, polyacrylic acid resins containing primary amino groups, and silicon-based resins containing primary amino groups. The resin base material and X(CH2) m Y and R a NHR b The molar ratio is 1:(0.5-4):(0.5-4).
7. Use of the nitrogen-containing heterocyclic resin according to any one of claims 1 to 4, characterized in that: Used for adsorbing metals, wherein the metal is any one or more of mercury, gallium, iron, cobalt, nickel, copper, zinc, lead, indium, cadmium, manganese, aluminum, uranium, vanadium, platinum group elements, gold, and silver.
8. The use according to claim 7, characterized in that The metal comprises one or more of cobalt, nickel, copper, zinc, cadmium, manganese and aluminum.
9. The use according to claim 8, characterized in that The metal includes one or more of nickel, copper and cobalt.
10. An adsorbent for solid phase extraction of metal elements, characterized in that: The adsorbent comprises the nitrogen-containing heterocyclic resin according to any one of claims 1 to 4.
11. A method for solid phase extraction of metal elements, characterized in that: Use of the adsorbent as claimed in claim 10.