Polyamide resin as well as preparation method and application thereof

By introducing polycyclic amine compounds into polyamide resins, the insufficient performance of alcohol-soluble polyamide resins under medium and high temperature conditions is solved, and good water resistance, heat resistance and adhesion are achieved, which improves its Application performance in high temperature and high humidity environments.

CN118930845AActive Publication Date: 2024-11-12WANHUA CHEM GRP CO LTD

Patent Information

Application Number
CN202411190654.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The existing alcohol-soluble polyamide resins are insufficient in medium and high temperature conditions, especially in high temperature and high humidity environments, and have poor water resistance and heat resistance, making it difficult to meet application needs.

Method used

Using amine compounds with a polycyclic structure, a polyamide resin with good alcohol solubility, water resistance and heat resistance is prepared through specific molar ratios and reaction steps to improve its hardness and adhesion.

Benefits of technology

While maintaining alcohol-soluble ability, the heat resistance, water resistance and mechanical strength of polyamide resin are significantly improved, and moisture absorption is avoided and application needs are met under medium and high temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930845A_ABST
    Figure CN118930845A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of polyamide resin, and particularly relates to polyamide resin and a preparation method and application thereof, and the polyamide resin comprises the following raw materials: a) carboxylic acid compounds; b) a polyamine compound; c) a compound with a structure as shown in the following formula (I); in the formula (I), R is selected from H or hydroxyl. The polyamide resin obtained by the preparation method disclosed by the invention not only has better alcohol solubility and water resistance, but also has higher heat resistance and better adhesion capability to a base material. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyamide resins, and in particular relates to a polyamide resin and a preparation method and application thereof. Background Art

[0002] Polyamide resin is mainly formed by the condensation of dibasic acid and diamine. Its molecular structure has a high density of amide bonds, which can give the material good bonding properties to metals, plastics, etc., excellent thermal stability and good resistance to chemical reagents. Polyamide ink is mainly used for gravure and letterpress printing inks, and is also an indispensable ink for printing packaging materials such as cellophane, polyethylene, and polypropylene films; polyamide hot melt adhesive is also a very important adhesive in the fields of textiles, footwear, etc.

[0003] As environmental protection requirements become increasingly stringent, alcohol-soluble polyamide resins have the advantages of low toxicity, environmental protection and high cost performance, and are slowly beginning to replace the more toxic benzene-soluble polyamide resins. However, the hardness, water resistance, adhesion to substrates, hygroscopicity, heat resistance and other properties of the alcohol-soluble polyamide resins currently prepared are all poor, making it difficult to meet the application requirements under medium and high temperature conditions, especially in the summer when the temperature is high and the humidity is high, and the problem of polyamide resin adhesion is more likely to occur.

[0004] In this regard, improvements and research have also been conducted in this field. For example, patent document CN103554486A prepares an alcohol-soluble dimer acid-type polyamide resin by using an ethanolamine modifier. However, ethanolamine is a small molecular aliphatic amine with strong hygroscopicity, which will lead to poor water resistance and heat resistance of the polyamide resin.

[0005] Therefore, in the research on polyamide resin modification, how to ensure that the polyamide resin has good alcohol solubility while also having strong water resistance, heat resistance and high adhesion is a technical difficulty. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a polyamide resin and a preparation method and application thereof. The obtained polyamide resin not only has good alcohol solubility, but also has good water resistance and high heat resistance, and has the advantages of good adhesion and bonding ability to substrates.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] In a first aspect, a polyamide resin is provided, which comprises the following raw materials:

[0009] a) carboxylic acid compounds;

[0010] b) polyamine compounds;

[0011] c) a compound having a structure shown in the following formula (I):

[0012]

[0013] In formula (I), R is selected from H or hydroxyl.

[0014] According to the polyamide resin provided by the present invention, in some embodiments, the ratio of the molar amount of carboxyl groups contained in component a) to the molar amount of primary amino groups contained in component b) and component c) is 1:(0.8-1.2), for example, 1:0.85, 1:0.9, 1:1, 1:1.05, 1:1.1, 1:1.15.

[0015] In some embodiments, the ratio of the molar amount of carboxyl groups contained in component a) to the molar amount of primary amino groups contained in components b) and c) is 1:(0.9-1.1), preferably 1:(0.95-1.05).

[0016] In some embodiments, the molar ratio of component b) to component c) is 1:(0.05-0.25), for example, 1:0.055, 1:0.06, 1:0.08, 1:0.1, 1:0.15, 1:0.2, 1:0.21, 1:0.22, 1:0.24, preferably 1:(0.05-0.2).

[0017] According to the polyamide resin provided by the present invention, in some embodiments, the carboxylic acid compound is selected from one or more of dimer acid, trimer acid, oleic acid, methyl oleate, adipic acid, sebacic acid, succinic acid and propionic acid.

[0018] In some embodiments, the polyamine compound is selected from one or more of ethylenediamine, hexamethylenediamine, decanediamine, pentamethylenediamine, methylpentamethylenediamine, isophoronediamine, 1,3-cyclohexanedimethylamine, 4,4'-diaminodicyclohexylmethane and polyetheramine.

[0019] In a second aspect, a method for preparing the polyamide resin as described above is provided, comprising the following steps:

[0020] 1) adding component a), component b) and component c) into a reaction vessel, heating the system to 100-140° C. (e.g., 105° C., 110° C., 115° C., 120° C., 125° C., 130° C., 135° C.) under the protection of an inert gas (e.g., nitrogen), and reacting at this temperature (e.g., reacting while stirring uniformly);

[0021] 2) While stirring and under the protection of an inert gas (such as nitrogen), the system is heated to 140-180° C. (for example, 145° C., 150° C., 155° C., 160° C., 165° C., 170° C., 175° C.), and the reaction is carried out at this temperature;

[0022] 3) While stirring and under the protection of an inert gas (such as nitrogen), the system is heated to 180-220° C. (for example, 185° C., 190° C., 195° C., 200° C., 205° C., 210° C., 215° C.), and the reaction is carried out at this temperature;

[0023] 4) While stirring and under the protection of an inert gas (such as nitrogen), the system is heated to 220-270° C. (for example, 225° C., 230° C., 235° C., 240° C., 245° C., 250° C., 255° C., 260° C., 265° C.), and the reaction is carried out at this temperature;

[0024] 5) After vacuum removal of water and unreacted small molecules in the system, the temperature is lowered and the material is discharged to obtain a polyamide resin.

[0025] According to the preparation method provided by the present invention, in some embodiments, the reaction time in step 1) is 0.5 to 2 h, for example, 1 h, 1.5 h, 1.8 h.

[0026] In some embodiments, the reaction time in step 2) is 1 to 3 h, for example, 1.5 h, 2 h, 2.5 h.

[0027] In some embodiments, the reaction time in step 3) is 1 to 3 h, for example, 1.5 h, 2 h, 2.5 h.

[0028] In some embodiments, the reaction time in step 4) is 1 to 3 h, for example, 1.5 h, 2 h, or 2.5 h.

[0029] In a third aspect, there is provided a use of the polyamide resin as described above or the polyamide resin prepared by the preparation method as described above in ink and hot melt adhesive.

[0030] Herein, the application steps or operation processes of the polyamide resin in ink and hot melt adhesive may be conventional operations in the art and will not be described in detail here.

[0031] Compared with the prior art, the technical solution of the present invention has at least the following beneficial effects:

[0032] Compared with the existing system, the present invention introduces an amine compound with a polycyclic structure into the polyamide resin. The polycyclic structure has a strong hydrophobic property. While maintaining a considerable alcohol solubility, it can improve the heat resistance and water resistance of the polyamide resin, and will not show obvious moisture absorption under high humidity conditions; at the same time, it can also improve the hardness and adhesion of the polyamide resin to a certain extent, thereby improving the mechanical strength of the polyamide resin.

[0033] For the system of introducing polycyclic amine compounds of the present invention, a hydroxyl-containing polycyclic amine compound is introduced into the polyamide resin, and while the polyamide resin maintains considerable hardness, water resistance, heat resistance and adhesion to various substrates, the alcohol solubility is further improved.

[0034] The compound with a polycyclic structure introduced into the polyamide resin of the present invention can be used in combination with a variety of diamines to prepare polyamide resins with different structures and different properties to meet the application needs of various occasions. DETAILED DESCRIPTION

[0035] In order to understand the technical features and content of the present invention in detail, the preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described in the embodiments, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. For those who do not specify specific conditions in the embodiments, they are carried out according to normal conditions or the conditions recommended by the manufacturer.

[0036] The names, abbreviations and sources of the main chemicals used in the embodiments of the present invention are shown in Table 1. Unless otherwise specified, all reagents used were of chemical analytical grade.

[0037] Table 1 Main raw material information

[0038] Chemical Name source Ethylenediamine, Hexamethylenediamine Inokay Dimer acid, oleic acid Shandong Huijin Isophorone diamine Wanhua Chemical 4,4'-Diaminodicyclohexylmethane Wanhua Chemical 4-(cyclohexylmethyl)cyclohexylamine; that is, in formula (I), R is H Wanhua Chemical 4-[(4-aminocyclohexyl)methyl]cyclohexanol; that is, in formula (I), R is -OH Wanhua Chemical

[0039] The main test methods used in the present invention are as follows:

[0040] (1) Hardness: Use a hardness tester to measure the Shore D hardness of the polyamide resin sample to be tested;

[0041] (2) Softening point: The softening point of the polyamide resin sample to be tested is tested in accordance with GB / T 1633-2017 "Resin Ring and Ball Softening Point Determination Method";

[0042] (3) Mechanical properties (peel strength): The polyamide resin to be tested was hot-melted and coated on the front and back sides of a clean iron sheet with a size of 20 mm*100 mm. A canvas of the same size was then pressed and attached to the iron sheet. After curing, the force required to pull the canvas apart was tested using a tensile tester.

[0043] (4) Water resistance test: Prepare the sample to be tested according to the method in point (3) above, then immerse it in water for 24 hours, and then perform the mechanical property test according to the description in point (3) above;

[0044] (5) Alcohol solubility test: The polyamide resin to be tested is dissolved in ethanol, and the viscosity of the polyamide resin ethanol solution at a solid content of 50% is tested; the lower the viscosity, the better the alcohol solubility.

[0045] [Example 1]

[0046] The preparation method of polyamide resin is:

[0047] 1) 1000 g of dimer acid (1.78 mol), 50 g of ethylenediamine (0.83 mol), 100 g of hexamethylenediamine (0.86 mol), and 40 g of 4-(cyclohexylmethyl)cyclohexylamine (0.2 mol) were added to a reaction vessel, and the system was heated to 100° C. under nitrogen protection, and stirred at this temperature for 0.5 h;

[0048] 2) Then, under stirring and nitrogen protection, the system was slowly heated to 140°C and kept at this temperature for 1 hour;

[0049] 3) Then, under stirring and nitrogen protection, the system was slowly heated to 180°C and kept at this temperature for 1 hour;

[0050] 4) Then, under stirring and nitrogen protection, the system was slowly heated to 220°C and kept at this temperature for 2 hours;

[0051] 5) Afterwards, the water and unreacted small molecules in the system are removed by vacuum, the temperature is lowered, and the material is discharged to obtain polyamide resin①.

[0052] [Example 2]

[0053] The preparation method of polyamide resin is:

[0054] 1) 1000 g of dimer acid (1.78 mol), 50 g of ethylenediamine (0.83 mol), 185 g of 4,4'-diaminodicyclohexylmethane (0.88 mol), and 16.5 g of 4-(cyclohexylmethyl)cyclohexylamine (0.09 mol) were added to a reaction vessel, and the system was heated to 120° C. under nitrogen protection, and stirred at this temperature for 1 hour;

[0055] 2) Then, under stirring and nitrogen protection, the system was slowly heated to 160°C and kept at this temperature for 2 hours;

[0056] 3) Then, under stirring and nitrogen protection, the system was slowly heated to 200°C and kept at this temperature for 1 hour;

[0057] 4) Then, under stirring and nitrogen protection, the system was slowly heated to 250°C and kept at this temperature for 3 hours;

[0058] 5) Afterwards, remove water and unreacted small molecules in the system by vacuum, cool down and discharge the material to obtain polyamide resin②.

[0059] [Example 3]

[0060] The preparation method of the polyamide resin is the same as that of Example 1, except that 4-(cyclohexylmethyl)cyclohexylamine in step 1) is replaced by 4-[(4-aminocyclohexyl)methyl]cyclohexanol; the remaining steps are the same as those of Example 1. Polyamide resin ③ is obtained.

[0061] [Example 4]

[0062] The preparation method of polyamide resin is similar to that of Example 2, except that 4-(cyclohexylmethyl)cyclohexylamine in step 1) is replaced by 4-[(4-aminocyclohexyl)methyl]cyclohexanol; the remaining steps are the same as those of Example 1. Polyamide resin ④ is obtained.

[0063] [Example 5]

[0064] The preparation method of polyamide resin is:

[0065] 1) 800 g of dimer acid (1.43 mol), 200 g of oleic acid (0.7 mol), 50 g of ethylenediamine (0.83 mol), 160 g of 4,4'-diaminodicyclohexylmethane (0.76 mol), and 66 g of 4-[(4-aminocyclohexyl)methyl]cyclohexanol (0.3 mol) were added to a reaction vessel, and the system was heated to 120° C. under nitrogen protection, and stirred at this temperature for 1 hour;

[0066] 2) Then, under stirring and nitrogen protection, the system was slowly heated to 180°C and kept at this temperature for 2 hours;

[0067] 3) Then, under stirring and nitrogen protection, the system was slowly heated to 220°C and kept at this temperature for 1 hour;

[0068] 4) Then, under stirring and nitrogen protection, the system was slowly heated to 270°C and kept at this temperature for 2 hours;

[0069] 5) Afterwards, remove water and unreacted small molecules in the system by vacuum, cool down and discharge the material to obtain polyamide resin ⑤.

[0070] [Example 6]

[0071] The preparation method of polyamide resin is:

[0072] 1) 800 g of dimer acid (1.43 mol), 200 g of oleic acid (0.7 mol), 100 g of hexamethylenediamine (0.86 mol), 150 g of isophoronediamine (0.88 mol), and 76 g of 4-[(4-aminocyclohexyl)methyl]cyclohexanol (0.36 mol) were added to a reaction vessel, and the system was heated to 120° C. under nitrogen protection, and stirred at this temperature for reaction for 1 hour;

[0073] 2) Then, under stirring and nitrogen protection, the system was slowly heated to 180°C and kept at this temperature for 2 hours;

[0074] 3) Then, under stirring and nitrogen protection, the system was slowly heated to 220°C and kept at this temperature for 2 hours;

[0075] 4) Then, under stirring and nitrogen protection, the system was slowly heated to 250°C and kept at this temperature for 2 hours;

[0076] 5) Afterwards, remove water and unreacted small molecules in the system by vacuum, cool down and discharge the material to obtain polyamide resin ⑥.

[0077] [Comparative Example 1] - Compared with Example 5

[0078] The preparation method of polyamide resin is:

[0079] 1) 800 g of dimer acid (1.43 mol), 200 g of oleic acid (0.7 mol), 50 g of ethylenediamine (0.83 mol), 160 g of 4,4'-diaminodicyclohexylmethane (0.76 mol), and 18.3 g of ethanolamine (0.3 mol) were added to a reaction vessel, and the system was heated to 120° C. under nitrogen protection, and stirred at this temperature for 1 hour;

[0080] 2) Then, under stirring and nitrogen protection, the system was slowly heated to 180°C and kept at this temperature for 2 hours;

[0081] 3) Then, under stirring and nitrogen protection, the system was slowly heated to 220°C and kept at this temperature for 1 hour;

[0082] 4) Then, under stirring and nitrogen protection, the system was slowly heated to 270°C and kept at this temperature for 2 hours;

[0083] 5) Afterwards, the water and unreacted small molecules in the system are removed by vacuum, the temperature is lowered, and the material is discharged to obtain polyamide resin ⑦.

[0084] [Comparative Example 2]

[0085] The preparation method of the polyamide resin is similar to that of Example 1, except that the amount of 4-(cyclohexylmethyl)cyclohexylamine is replaced with 3.9 g (0.02 mol); the remaining steps are the same as those of Example 1; and the polyamide resin⑧ is obtained.

[0086] [Comparative Example 3]

[0087] The preparation method of the polyamide resin is similar to that of Example 1, except that the amount of 4-(cyclohexylmethyl)cyclohexylamine is replaced with 58.2 g (0.3 mol); the remaining steps are the same as those of Example 1; and polyamide resin ⑨ is obtained.

[0088] The performance of the polyamide resins obtained in the embodiments and comparative examples was tested, and the results are shown in Table 2:

[0089] Table 2 Polyamide resin performance test results

[0090]

[0091] It can be seen from the above test results that, under the condition of equivalent alcohol solubility, the polyamide resin in the embodiment of the present invention has higher heat resistance and higher hardness, and at the same time has better adhesion and bonding properties on the surface of the substrate, thereby making it have excellent mechanical properties; that is, the alcohol solubility of the obtained polyamide resin can be balanced with hardness, heat resistance, water resistance and bonding properties, and it has high practical value.

[0092] Compared with Example 1-2, Example 3-4 introduces a hydroxyl-containing polycyclic amine compound into the polyamide resin, which has certain advantages in alcohol solubility while maintaining comparable properties of the polyamide resin such as hardness, water resistance, heat resistance, and adhesion.

[0093] Compared with Comparative Example 1 in which no polycyclic amine compound is introduced, Example 5 introduces a polycyclic amine compound into the polyamide resin, which can improve the hardness, water resistance, and heat resistance of the polyamide resin while maintaining a considerable alcohol solubility, and improve the adhesion of the polyamide resin on various substrates.

[0094] In Comparative Example 2-3, although a polycyclic amine compound was added, its amount was not controlled within an appropriate range, and a balance between the alcohol solubility and the hardness, heat resistance, water resistance, and adhesion of the obtained polyamide resin could not be achieved.

[0095] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the spirit of the present invention.

Claims

1. A polyamide resin, characterized in that It includes the following raw material components: a) carboxylic acid compounds; b) polyamine compounds; c) a compound having a structure shown in the following formula (I): In formula (I), R is selected from H or hydroxyl.

2. The polyamide resin according to claim 1, characterized in that The ratio of the molar amount of carboxyl groups contained in component a) to the molar amount of primary amino groups contained in components b) and c) is 1:(0.8-1.2).

3. The polyamide resin according to claim 1 or 2, characterized in that The ratio of the molar amount of carboxyl groups contained in component a) to the molar amount of primary amino groups contained in components b) and c) is 1:(0.9-1.1), preferably 1:(0.95-1.05).

4. The polyamide resin according to any one of claims 1 to 3, characterized in that The molar ratio of component b) to component c) is 1:(0.05-0.25), preferably 1:(0.05-0.2).

5. The polyamide resin according to any one of claims 1 to 4, characterized in that The carboxylic acid compound is selected from one or more of dimer acid, trimer acid, oleic acid, methyl oleate, adipic acid, sebacic acid, succinic acid and propionic acid.

6. The polyamide resin according to any one of claims 1 to 5, characterized in that The polyamine compound is selected from one or more of ethylenediamine, hexamethylenediamine, decanediamine, pentamethylenediamine, methylpentamethylenediamine, isophoronediamine, 1,3-cyclohexanedimethylamine, 4,4'-diaminodicyclohexylmethane and polyetheramine.

7. The method for preparing a polyamide resin according to any one of claims 1 to 6, characterized in that: The following steps are involved: 1) Add component a), component b) and component c) into a reaction container, and under the protection of inert gas, heat the system to 100-140° C. and react at this temperature; 2) While stirring and under the protection of inert gas, the system is heated to 140-180°C and kept at this temperature for reaction; 3) While stirring and under the protection of inert gas, the system is heated to 180-220°C and kept at this temperature for reaction; 4) While stirring and under the protection of inert gas, the system is heated to 220-270°C and kept at this temperature for reaction; 5) After vacuum removal of water and unreacted small molecules in the system, the temperature is lowered and the material is discharged to obtain a polyamide resin.

8. The preparation method according to claim 7, characterized in that: The reaction time in step 1) is 0.5 to 2 hours.

9. The preparation method according to claim 7 or 8, characterized in that: The reaction time in step 2) is 1 to 3 hours; The reaction time in step 3) is 1 to 3 hours; The reaction time in step 4) is 1 to 3 hours.

10. Use of the polyamide resin according to any one of claims 1 to 6 or the polyamide resin prepared by the preparation method according to any one of claims 7 to 9 in inks and hot melt adhesives.

Citation Information

Patent Citations

  • Polyamide resin and preparation method thereof and polyamide material prepared from same

    CN106188534A

  • Aliphatic transparent polyamide preparation method and aliphatic transparent polyamide

    CN106916296A

  • Imide film and synthesis method thereof

    CN113881225A

  • Polyamide resin

    JP2002284872A

  • Method For Producing An Aqueous Polyamide Dispersion

    US20080275182A1

Cited By

  • Alcohol-soluble polyamide resin for printing ink as well as preparation method and application of alcohol-soluble polyamide resin

    CN120059174A

  • An alcohol-soluble polyamide resin for ink, its preparation method and application

    CN120059174B