Polar hybridization modified high-humidity non-slip rubber sole material and preparation method thereof

Through polar hybrid modified rubber and emulsion blending technology, combined with sodium borate crosslinking and vulcanization technology, the polarity and surface roughness of rubber sole materials are improved, and the problem of insufficient anti-slip performance on slippery ground is solved, and the problem of insufficient anti-slip performance on slippery ground is achieved. The dual performance of high humidity, anti-slip and wear resistance is improved to meet the needs of high-intensity exercise.

CN118930989APending Publication Date: 2024-11-12QIAODAN SPORTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411266992.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing rubber sole material has insufficient anti-slip performance on slippery ground, making it difficult to meet the needs of high-intensity sports such as running and outdoor off-roading scenarios.

Method used

By increasing the polarity and surface roughness of the rubber material, polar hybrid modified rubber and emulsion blending technology is used, combined with sodium borate crosslinking and vulcanization technology, high humidity anti-slip rubber sole material is prepared to improve the rubber and the ground Contact area and grip.

Benefits of technology

It significantly improves the wet anti-slip performance of rubber sole material, while maintaining good wear resistance, meeting the needs of high-end sports shoes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a polar hybrid modified high-humidity non-slip rubber sole material and a preparation method thereof, and the polar hybrid modified high-humidity non-slip rubber sole material comprises the following components by mass: 40-60 PHR of polybutadiene rubber, 10-20 PHR of brominated butyl rubber, 30-40 PHR of polar hybrid modified rubber, 30-50 PHR of white carbon black, 2-4 PHR of a silane coupling agent, 2-4 PHR of polyethylene glycol, 3-5 PHR of activated zinc oxide, 0.5-0.7 PHR of stearic acid, 1-2 PHR of an anti-aging agent, 3-5 PHR of a plasticizer, 1.5-2.0 PHR of a bridging agent, and 0.5-1.5 PHR of an accelerator. According to the invention, polyvinyl alcohol is introduced into a rubber formula system for hybridization modification by adopting an emulsion mixing mode, so that the polarity and surface roughness of the rubber sole material are improved, and the wet non-slip performance of the rubber sole material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rubber sole materials, and particularly relates to a high-humidity anti-skid rubber sole material modified by polar hybridization and a preparation method thereof. Background Art

[0002] Rubber outsoles are wear-resistant and anti-slip, and are widely used in sports shoes to provide grip and improve durability. With the popularity of high-intensity sports such as running and outdoor cross-country, people's demand for the functionality of sports shoes is also increasing. Rubber outsoles need to have higher wear resistance and better wet anti-slip properties. From the perspective of wet and slippery interface contact, increasing the polarity and roughness of the rubber material surface is conducive to increasing the contact area between the rubber and the ground. At the same time, it can better pierce the water film layer on wet and slippery ground, achieving direct contact between the rubber and the substrate, thereby improving the anti-slip performance.

[0003] In view of this, the present invention proposes a high-wetness anti-skid rubber sole material modified by polar hybridization and a preparation method thereof, which improves the wet anti-skid performance of the rubber sole material by increasing the polarity and surface roughness of the rubber. Summary of the invention

[0004] To achieve the above object, the present invention adopts the following technical scheme: a high-humidity anti-slip rubber sole material modified by polar hybridization, comprising the following components in parts by mass: Polybutadiene rubber 40-60PHR, brominated butyl rubber 10-20PHR, polar hybrid modified rubber 30-40PHR, white carbon black 30-50PHR, silane coupling agent 2-4PHR, polyethylene glycol 2-4PHR, active zinc oxide 3-5PHR, stearic acid 0.5-0.7PHR, antioxidant 1-2PHR, plasticizer 3-5PHR, bridging agent 1.5-2.0PHR, accelerator 0.5-1.5PHR.

[0005] Furthermore, the polar hybrid modified rubber is prepared by blending PVA and rubber latex, adding sodium borate water solution, gelling, and then freeze-drying. According to the solid mass, ω(PVA):ω(rubber latex solid content)=1:(4-8), and the sodium borate for cross-linking is 1% of the mass of PVA; Furthermore, the polybutadiene rubber is butadiene rubber with a high cis 1'4 structure.

[0006] Furthermore, the bromine content of the brominated butyl rubber is 1.80±0.20%.

[0007] Furthermore, the white carbon black has a specific surface area of ​​250 to 260 m 2 / g high specific surface area white carbon black.

[0008] Furthermore, the coupling agent is a sulfur-containing silane coupling agent.

[0009] Furthermore, the antioxidant is a hindered phenol antioxidant.

[0010] Furthermore, the plasticizer is heavy cycloalkane oil.

[0011] Furthermore, the bridging agent is insoluble sulfur.

[0012] Furthermore, the accelerator is one or more of thiazoles, thiurams or sulfenamides.

[0013] The present invention also provides a method for preparing a high-humidity anti-slip rubber sole material modified by polar hybridization, which comprises the following steps according to the above material components: (1) Weigh polybutadiene rubber, brominated butyl rubber, polar hybrid modified rubber, active zinc oxide, stearic acid, antioxidant, and plasticizer and pour them into a banbury mixer for kneading at a temperature of 100 to 115°C for 2 to 3 minutes; (2) Weigh white carbon black, polyethylene glycol and coupling agent and pour them into a banbury mixer for mixing. Mix them together with the mixed rubber material at a mixing temperature of 130-135°C for 3-4 minutes. (3) The mixed material obtained in step (2) is cooled by a water machine and then stored in sheets; (4) adding a bridging agent, a bridging aid and a colorant to the bulk material obtained in step (3) on a wheel platform and performing refining for 6 to 10 minutes to uniformly mix the bulk material to obtain a mixture; (5) Cutting the mixed material in step (4) and subjecting it to flat-plate compression vulcanization in a mold at a vulcanization temperature of 155 to 165° C. for a vulcanization time of 180 to 210 seconds to obtain a finished rubber sole material.

[0014] By adopting the above technical scheme, the beneficial effects of the present invention are: through the reasonable combination of rubber formulas, polyvinyl alcohol is introduced into the rubber formula system by emulsion mixing to perform hybrid modification, thereby increasing the polarity and surface roughness of the rubber, thereby improving the wet anti-slip performance of the rubber sole material. DETAILED DESCRIPTION

[0015] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0016] The present invention provides a high-humidity anti-slip rubber sole material modified by polar hybridization, and the formula material includes the following raw materials in parts by mass: Polybutadiene rubber 40-60PHR, brominated butyl rubber 10-20PHR, polar hybrid modified rubber 30-40PHR, white carbon black 30-50PHR, silane coupling agent 2-4PHR, polyethylene glycol 2-4PHR, active zinc oxide 3-5PHR, stearic acid 0.5-0.7PHR, antioxidant 1-2PHR, plasticizer 3-5PHR, bridging agent 1.5-2.0PHR, accelerator 0.5-1.5PHR.

[0017] The high-wet anti-skid rubber sole material provided by the present invention has excellent wet anti-skid performance and good wear resistance, and meets the sole performance requirements of high-intensity sports such as running and outdoor cross-country.

[0018] The polybutadiene rubber is a butadiene rubber with a high cis 1'4 structure, and its brand number is BR9000.

[0019] The bromine content of the brominated butyl rubber is 1.80±0.20%, and its brand is BIIR X2, produced by Lanxess, Germany.

[0020] The polar hybrid modified rubber is prepared by blending PVA and rubber latex, dissolving in sodium borate water solution, and then freeze-drying.

[0021] PVA (polyvinyl alcohol) is a polymer with strongly polar functional groups, hydroxyl groups, which is obtained by hydrolysis of polyvinyl acetate. It has good hydrophilicity, is soluble in water, and has good mechanical properties. Its strength is further improved by cross-linking with boric acid. The rubber material for the sole is usually a non-polar or weakly polar polymer with poor hydrophilicity. Through emulsion blending, it can be better introduced and dispersed in the rubber matrix, and the molecular chains are entangled with each other. PVA is cross-linked with sodium borate, so that the rubber molecular chains pass through the PVA cross-linking network, increasing the roughness and polarity of the rubber matrix surface. Compared with petroleum anti-slip resins, it can better drain water film and greatly improve the wet anti-slip performance of rubber.

[0022] The specific preparation method of the polar hybrid modified rubber is as follows: (1) Weigh a certain amount of PVA powder, add it into a certain amount of water under mechanical stirring, and wait for it to be completely dissolved to prepare a PVA aqueous solution; (2) Weigh the rubber latex and slowly add it to the above PVA aqueous solution, according to the solid content, ω(PVA):ω(rubber latex solid content) = 1:(4-8), and continue stirring for 2 hours; (3) Under stirring, the PVA emulsion of step (2) is slowly added to a 1% by mass sodium borate aqueous solution to obtain a mixture gel, wherein, according to the solid content, according to the solid mass, ω(PVA):ω(rubber emulsion solid content)=1:(4-8), and the sodium borate having a cross-linking effect is 1% by mass of the PVA; (4) The obtained gel is freeze-dried in vacuum to obtain polar hybrid modified rubber.

[0023] Furthermore, the rubber latex in step (2) is one or both of natural rubber and carboxylated nitrile rubber latex, wherein the solid content of the natural rubber latex is 60%, and the solid content of the carboxylated nitrile rubber latex is 45%. In terms of solid content, ω (carboxylated nitrile rubber): ω (natural rubber) = 1: (1-5), preferably 1:3.

[0024] The white carbon black is a high specific surface area white carbon black, with a specific surface area of ​​250-260m 2 / g, model JS-260, produced by Fujian Jinsha Silica Co., Ltd.

[0025] The coupling agent is a sulfur-containing silane coupling agent, and its brand is Si-69.

[0026] The brand of the polyethylene glycol is PEG4000.

[0027] The antioxidant is a hindered phenol antioxidant, and its brand is AO-80; it is a polar macromolecule that can increase the interaction between PVA and rubber matrix molecules, improve the damping performance of the material, thereby increasing the 0°C loss factor and improving the wet anti-slip performance of the rubber material.

[0028] The plasticizer is heavy cycloalkane oil, and its brand is 4006.

[0029] The bridging agent is insoluble sulfur.

[0030] The accelerator is one or more of thiazoles, thiurams or sulfonamides, wherein the thiazole is DM, the thiurams are TT, and the sulfonamides are CZ.

[0031] There is no special requirement for the active zinc oxide and stearic acid, and conventional commercially available ones can be used.

[0032] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention. In the present invention, unless otherwise stated, the amounts involved in the present invention are all mass percentages. Example 1

[0033] A high-humidity anti-skid rubber sole material modified by polar hybridization, comprising the following raw materials by weight: 60 PHR of butadiene rubber (BR9000), 10 PHR of brominated butyl rubber (BIIR X2), 30 PHR of polar hybrid modified rubber, 40 PHR of white carbon black (JS260), 4 PHR of silane coupling agent (Si-69), 3 PHR of polyethylene glycol (PEG4000), 3 PHR of active zinc oxide, 0.5 PHR of stearic acid, 2 PHR of antioxidant (AO-80), 3 PHR of plasticizer (naphthenic oil 4006), 2.0 PHR of bridging agent (insoluble sulfur), 1.0 PHR of accelerator (DM), 0.1 PHR of accelerator (TT), and 0.5 PHR of accelerator (CZ). Example 2

[0034] A high-humidity anti-skid rubber sole material modified by polar hybridization, comprising the following raw materials by weight: 55 PHR of butadiene rubber (BR9000), 10 PHR of brominated butyl rubber (BIIR X2), 35 PHR of polar hybrid modified rubber, 40 PHR of white carbon black (JS260), 4 PHR of silane coupling agent (Si-69), 3 PHR of polyethylene glycol (PEG4000), 3 PHR of active zinc oxide, 0.5 PHR of stearic acid, 2 PHR of antioxidant (AO-80), 3 PHR of plasticizer (naphthenic oil 4006), 2.0 PHR of bridging agent (insoluble sulfur), 1.0 PHR of accelerator (DM), 0.1 PHR of accelerator (TT), and 0.5 PHR of accelerator (CZ). Example 3

[0035] A high-humidity anti-skid rubber sole material modified by polar hybridization, comprising the following raw materials by weight: 50 PHR of butadiene rubber (BR9000), 10 PHR of brominated butyl rubber (BIIR X2), 40 PHR of polar hybrid modified rubber, 40 PHR of white carbon black (JS260), 4 PHR of silane coupling agent (Si-69), 3 PHR of polyethylene glycol (PEG4000), 3 PHR of active zinc oxide, 0.5 PHR of stearic acid, 2 PHR of antioxidant (AO-80), 3 PHR of plasticizer (naphthenic oil 4006), 2.0 PHR of bridging agent (insoluble sulfur), 1.0 PHR of accelerator (DM), 0.1 PHR of accelerator (TT), and 0.5 PHR of accelerator (CZ).

[0036] A method for preparing a high-humidity anti-slip rubber sole material modified by polar hybridization, wherein the raw materials are added according to the above ratio, and the method comprises the following steps: (1) Preparation of polar hybrid modified rubber: 1) Weigh 10 g of PVA 2488 powder, add it into 90 g of water under mechanical stirring, continue stirring until it is completely dissolved, and prepare a PVA aqueous solution with a mass fraction of 10%; 2) Weigh 62.5 g of natural rubber latex and 27.8 g of carboxylated nitrile rubber latex and slowly add them into the beaker in 1), and continue stirring for 2 h; 3) While stirring, slowly add 10 g of 1% sodium borate aqueous solution to obtain a gel solid; 4) vacuum freeze-drying the gel solid obtained in 3) to obtain a polar hybrid modified rubber; (2) Weigh polybutadiene rubber, brominated butyl rubber, polar hybrid modified rubber, active zinc oxide, stearic acid, antioxidant, and plasticizer into a banbury mixer and mix them at a temperature of 100 to 115°C for 2 to 3 minutes; (3) Weigh white carbon black, polyethylene glycol and coupling agent and pour them into a banbury mixer for mixing. Mix them together with the mixed rubber material at a mixing temperature of 130-135°C for 3-4 minutes. (4) cooling the mixture obtained in step (3) through a water machine, discharging the mixture into sheets and storing them; (5) adding a bridging agent, a bridging aid and a colorant to the large flakes obtained in step (4) on a wheel platform and kneading for 6 to 10 minutes to uniformly obtain a mixture; (6) Cutting the mixed material in step (5) and subjecting it to flat-plate compression vulcanization in a mold at a vulcanization temperature of 155 to 165° C. for a vulcanization time of 180 to 210 seconds to obtain a finished rubber sole material. Comparative Example

[0037] A non-slip rubber material, comprising the following raw materials in parts by mass: Butadiene rubber (BR9000) 50 PHR, brominated butyl rubber (BIIR X2) 10 PHR, natural rubber 30 PHR, carboxylated nitrile rubber 10 PHR, petroleum anti-slip resin 8 PHR, white carbon black (JS260) 40 PHR, silane coupling agent (Si-69) 4 PHR, polyethylene glycol (PEG4000) 3 PHR, active zinc oxide 3 PHR, stearic acid 0.5 PHR, antioxidant (AO-80) 2 PHR, plasticizer (naphthenic oil 4006) 3 PHR, bridging agent (insoluble sulfur) 2.0 PHR, accelerator (DM) 1.0 PHR, accelerator (TT) 0.1 PHR, accelerator (CZ) 0.5 PHR.

[0038] The natural rubber grade is 3L, produced by Vietnam Dajinbei; the carboxylated nitrile rubber grade is X146, produced by Germany Lanxess; the petroleum anti-slip resin is C9 petroleum resin, produced by Shandong Ningsong Chemical; and the remaining other materials are the same as those in the embodiment.

[0039] The method for preparing the above-mentioned anti-slip rubber material comprises the following steps: (1) Weigh polybutadiene rubber, brominated butyl rubber, natural rubber, carboxylated nitrile rubber, petroleum anti-slip resin, active zinc oxide, stearic acid, antioxidant, and plasticizer into a banbury mixer and mix at a temperature of 100 to 115°C for 2 to 3 minutes; (2) Weigh white carbon black, polyethylene glycol and coupling agent and pour them into a banbury mixer for mixing. Mix them together with the mixed rubber material at a mixing temperature of 130-135°C for 3-4 minutes. (3) The mixed material obtained in step (2) is cooled by a water machine and then stored in sheets; (4) adding a bridging agent, a bridging aid and a colorant to the bulk material obtained in step (3) on a wheel platform and performing refining for 6 to 10 minutes to uniformly mix the bulk material to obtain a mixture; (5) Cutting the mixed material in step (4) and subjecting it to flat-plate compression vulcanization in a mold at a vulcanization temperature of 155 to 165° C. for a vulcanization time of 180 to 210 seconds to obtain a finished rubber sole material.

[0040] The physical properties of the shoe sole materials obtained in the above examples and comparative examples were tested, and the results are shown in the following table.

[0041]

[0042] From the results in the above table, we can see that with the addition of polar hybrid modified rubber, compared with the petroleum anti-slip resin control group, the wet anti-slip performance increases and the wear resistance decreases slightly, but the wear resistance and other properties of the sole are still within the standard range. The performance advantage is obvious and can meet the wear resistance and anti-slip requirements of high-end sports shoes.

[0043] The above is a detailed introduction to the high-humidity anti-slip rubber sole material modified by polar hybridization and its preparation method provided by the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention, and these improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A high-humidity non-slip rubber sole material modified by polar hybridization, comprising the following components by mass: 40-60 PHR of polybutadiene rubber, 10-20 PHR of bromobutyl rubber, 30-40 PHR of polar hybrid modified rubber, 30-50 PHR of white carbon black, 2-4 PHR of silane coupling agent, 2-4 PHR of polyethylene glycol, 3-5 PHR of active zinc oxide, 0.5-0.7 PHR of stearic acid, 1-2 PHR of antioxidant, 3-5 PHR of plasticizer, 1.5-2.0 PHR of bridging agent, and 0.5-1.5 PHR of accelerator; The polar hybrid modified rubber is prepared by blending PVA and rubber latex, gelling with sodium borate aqueous solution, and then freeze-drying in vacuo, wherein according to the solid mass, ω(PVA):ω(rubber latex solid content)=1:(4-8), and the sodium borate for cross-linking is 1% of the mass of PVA; The polybutadiene rubber is a butadiene rubber with a high cis-1'4 structure; the bromine content of the brominated butyl rubber is 1.80±0.20%.

2. The high-humidity anti-slip rubber sole material modified by polar hybridization as claimed in claim 1, characterized in that The white carbon black has a specific surface area of ​​250 to 260 m 2 / g high specific surface area white carbon black.

3. The high-humidity anti-slip rubber sole material modified by polar hybridization as claimed in claim 1, characterized in that The coupling agent is a sulfur-containing silane coupling agent; the antioxidant is a hindered phenol antioxidant; the plasticizer is a heavy cycloalkane oil; and the bridging agent is insoluble sulfur.

4. The high-humidity anti-slip rubber sole material modified by polar hybridization as claimed in claim 1, characterized in that The accelerator is one or more of thiazoles, thiurams or sulfenamides.

5. A method for preparing a high-humidity anti-slip rubber sole material modified by polar hybridization according to any one of claims 1 to 4, comprising the following steps: (1) Weigh polybutadiene rubber, brominated butyl rubber, polar hybrid modified rubber, active zinc oxide, stearic acid, antioxidant, and plasticizer and pour them into a banbury mixer for kneading at a temperature of 100 to 115°C for 2 to 3 minutes; (2) Weigh white carbon black, polyethylene glycol and coupling agent and pour them into a banbury mixer for mixing. Mix them together with the mixed rubber material at a mixing temperature of 130-135°C for 3-4 minutes. (3) The mixed material obtained in step (2) is cooled by a water machine and then stored in sheets; (4) adding a bridging agent, a bridging aid and a colorant to the bulk material obtained in step (3) on a wheel platform and performing refining for 6 to 10 minutes to uniformly mix the bulk material to obtain a mixture; (5) Cutting the mixed material in step (4) and subjecting it to flat-plate compression vulcanization in a mold at a vulcanization temperature of 155 to 165° C. for a vulcanization time of 180 to 210 seconds to obtain a finished rubber sole material.

6. The method for preparing a high-humidity anti-slip rubber sole material modified by polar hybridization as claimed in claim 5, characterized in that The preparation method of the polar hybrid modified rubber comprises the following steps: (1) Weigh a certain amount of PVA powder, add it into a certain amount of water under mechanical stirring, wait for it to be completely dissolved, and prepare a PVA aqueous solution with a mass fraction of 10%; (2) Weigh the rubber latex and slowly add it to the above PVA aqueous solution, according to the solid content, ω(PVA):ω(rubber latex solid content) = 1:(4-8), and continue stirring for 2 hours; (3) under stirring, slowly adding the PVA emulsion of step (2) into a 1% by mass sodium borate aqueous solution to obtain a mixture gel, wherein the mass of the sodium borate is 1% of the mass of the PVA in terms of solid content; (4) The obtained gel is freeze-dried in vacuum to obtain polar hybrid modified rubber.

7. The method for preparing the polar hybrid modified rubber according to claim 6, characterized in that The rubber latex in step (2) is one or both of natural rubber and carboxylated nitrile rubber latex, wherein the solid content of the natural rubber latex is 60%, and the solid content of the carboxylated nitrile rubber latex is 45%. According to the solid content, ω (carboxylated nitrile rubber): ω (natural rubber) = 1: (1-5).