Silicon dioxide composite slurry as well as preparation method and application thereof

By modifying the combination of silica and silazane by silane coupling agent, a spherical silica composite slurry is formed, which solves the problem of inorganic filler settlement in epoxy potting glue and achieves low viscosity and high fluidity epoxy Potting adhesive improves product stability and performance consistency.

CN118931420APending Publication Date: 2024-11-12NOVORAY (LIANYUNGANG) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411268241.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Inorganic fillers in epoxy potting adhesives are prone to settle, resulting in poor consistency, which affects the performance of the terminal products. The viscosity increases or dispersion after the prior art is added to the anti-deposition agent, making it difficult to maintain low viscosity and high fluidity.

Method used

Silica is modified with silane coupling agent, combined with silazane and acid anhydride, and spherical silica composite slurry is formed through surface treatment and secondary modification, to improve the dispersion and anti-settlement properties of the filler, and add epoxy filling to seal Keep low viscosity and high fluidity after glue.

Benefits of technology

The good dispersion of silica composite slurry in epoxy potting glue is achieved, avoiding settlement, maintaining low viscosity and high fluidity, and improving product stability and performance consistency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005039430770000101
    Figure BDA0005039430770000101
Patent Text Reader

Abstract

The invention provides silicon dioxide composite slurry as well as a preparation method and application thereof. The small-particle-size spherical silicon dioxide is adopted as the raw material, and the silane coupling agent is used for surface treatment, so that the problem that the filler is easy to settle in the use process can be improved, and the filler is prevented from settling in the placement process after being added into the epoxy pouring sealant. Meanwhile, silazane is added in the preparation process of the slurry for secondary modification, the silazane can react with hydroxyl groups on the surface of silicon dioxide, the content of the hydroxyl groups on the surface of the silicon dioxide is reduced, and therefore the thixotropy of the silicon dioxide is improved; the preparation method comprises the following steps: adding acid anhydride to form composite slurry, and after the composite slurry is added into the epoxy pouring sealant, small-particle-size spherical silicon dioxide and micron-sized silicon dioxide are matched for use, so that the epoxy pouring sealant has low viscosity and high flowability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of potting glue, and in particular to a silicon dioxide composite slurry and a preparation method and application thereof. Background Art

[0002] Epoxy potting glue refers to a type of epoxy resin liquid packaging or potting material made of epoxy resin as the main component, various functional additives added, and a suitable curing agent. Due to the superior properties of epoxy resin, epoxy resin potting glue is also widely used. At the same time, in order to further improve the modulus, expansion coefficient, thermal conductivity and other properties of epoxy potting glue, it is necessary to add inorganic fillers such as silicon micropowder and alumina. Due to the density difference between inorganic fillers and organic components, the epoxy potting glue with pre-added inorganic fillers will have problems such as easy sedimentation of inorganic fillers and bottom hardening during storage, resulting in poor consistency of epoxy potting glue, resulting in the physical properties of the final epoxy potting glue deviating from the design value, and causing the failure of the terminal product.

[0003] In order to improve the sedimentation of epoxy potting glue, thixotropic organic anti-settling agents, inorganic anti-settling agents, etc. can be added. For example, the existing patent with publication number CN116606619A discloses a method for preparing a one-component epoxy resin glue electronic potting glue, by adding an organic anti-settling agent BYK-410. However, this will increase the viscosity of the epoxy potting glue and affect the fluidity of the epoxy potting glue product. The sedimentation can also be improved by adding a small-particle-size nano inorganic filler (such as fumed silica). For example, the existing patent with publication number CN111087942A discloses an additive composition for potting glue and its application, by adding fumed silica and inorganic anti-settling agent bentonite to improve the sedimentation, but fumed silica is not easy to disperse, and higher requirements are also put forward for the dispersion equipment. At the same time, due to the large specific surface area of ​​fumed silica, it will also cause the problem of increased viscosity and large thixotropy during use.

[0004] Therefore, there is an urgent need for a silica material that is easy to disperse, has good anti-settling performance, has low thixotropy, and can keep the potting compound at low viscosity and high fluidity. Summary of the invention

[0005] The purpose of the present invention is to provide a silicon dioxide composite slurry and its preparation method and application. The silicon dioxide composite slurry provided by the present invention is easy to disperse, has good anti-settling performance, and has small thixotropy. After being added to epoxy potting glue, the epoxy potting glue can maintain low viscosity and high fluidity.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The invention provides a silicon dioxide composite slurry, which is prepared by the following raw materials: silicon dioxide modified by a silane coupling agent, silazane, an acid anhydride and a promoter; the mass ratio of the silazane to the silicon dioxide modified by the silane coupling agent is (0.1-0.5):100; the mass ratio of the acid anhydride to the silicon dioxide modified by the silane coupling agent is (3-8):(3-8); the mass ratio of the promoter to the acid anhydride is (0.2-2.0):100; the silicon dioxide in the silicon dioxide modified by the silane coupling agent is spherical; the D50 of the silicon dioxide is 0.1-2.0 μm; the D100 of the silicon dioxide is ≤8.0 μm; the specific surface area of ​​the silicon dioxide is 3.0-20 m 2 / g.

[0008] Preferably, the silane coupling agent in the silane coupling agent-modified silica includes one or more of anilinosilane, alkylsilane, epoxysilane and vinylsilane.

[0009] Preferably, the silazane includes one or both of hexamethyldisilazane and tetramethyldisilazane.

[0010] Preferably, the acid anhydride comprises one or both of methyltetrahydrophthalic anhydride and methylhexahydrophthalic anhydride.

[0011] Preferably, the accelerator comprises one or more of a tertiary amine accelerator and an imidazole accelerator. The present invention also provides a method for preparing the silicon dioxide composite slurry described in the above technical solution, comprising the following steps:

[0012] (1) performing a first modification on silicon dioxide using a silane coupling agent to obtain silicon dioxide modified with a silane coupling agent;

[0013] (2) The silane coupling agent-modified silica obtained in step (1) is mixed with silazane, anhydride and a promoter, and then subjected to a second modification to obtain a silica composite slurry.

[0014] Preferably, in step (1), the mass ratio of the silane coupling agent to silicon dioxide is (0.2-2):100.

[0015] Preferably, the temperature of the first modification in step (1) is 80 to 150° C., and the time of the first modification is 20 to 60 minutes.

[0016] Preferably, the temperature of the second modification in step (2) is 50 to 90° C., and the time of the second modification is 20 to 60 minutes.

[0017] The present invention also provides the use of the silicon dioxide composite slurry described in the above technical solution or the silicon dioxide composite slurry prepared according to the preparation method described in the above technical solution in epoxy potting glue.

[0018] The invention provides a silicon dioxide composite slurry, which is prepared by the following raw materials: silicon dioxide modified by a silane coupling agent, silazane, an acid anhydride and a promoter; the mass ratio of the silazane to the silicon dioxide modified by the silane coupling agent is (0.1-0.5):100; the mass ratio of the acid anhydride to the silicon dioxide modified by the silane coupling agent is (3-8):(3-8); the mass ratio of the promoter to the acid anhydride is (0.2-2.0):100; the silicon dioxide in the silicon dioxide modified by the silane coupling agent is spherical; the D50 of the silicon dioxide is 0.1-2.0 μm; the D100 of the silicon dioxide is ≤8.0 μm; the specific surface area of ​​the silicon dioxide is 3.0-20 m 2 / g. The present invention limits the shape and particle size of silica, uses spherical silica with a small particle size as a raw material, and uses a silane coupling agent for surface treatment, thereby improving the problem of easy sedimentation of the filler and avoiding sedimentation during placement after being added to the epoxy potting glue. At the same time, silazane is added during the preparation of the slurry for secondary modification. Silazane can also react with hydroxyl groups on the surface of silica to reduce the hydroxyl content on the surface of silica, thereby improving its thixotropy. Acid anhydride is added to form a composite slurry. After being added to the epoxy potting glue, the small-particle spherical silica and micron-sized silica are used in combination, so that the epoxy potting glue has low viscosity and high fluidity. The results of the embodiment show that the viscosity of the silica composite slurry provided by the present invention is below 881cp, the thixotropy is below 1.50, and it is placed at 60°C for 7 days without stratification and no sediment at the bottom. After adding it to the epoxy potting glue component B, the viscosity of the epoxy potting glue component B is 536cp, the thixotropy is 1.13, and it is placed at 60°C for 7 days without stratification and no sediment at the bottom. DETAILED DESCRIPTION

[0019] The invention provides a silicon dioxide composite slurry, which is prepared by comprising the following raw materials: silane coupling agent modified silicon dioxide, silazane, acid anhydride and accelerator.

[0020] Unless otherwise specified, the present invention has no particular limitation on the sources of the raw materials, and commercially available products known to those skilled in the art may be used.

[0021] The raw materials for preparing the silicon dioxide composite slurry of the present invention include silicon dioxide modified by a silane coupling agent.

[0022] In the present invention, the silica in the silane coupling agent modified silica is preferably spherical; the D50 of the silica is preferably 0.1 to 2.0 μm; the D100 of the silica is preferably ≤ 8.0 μm; the specific surface area of ​​the silica is preferably 3.0 to 20.0 m 2 The present invention limits the shape, particle size and specific surface area of ​​silicon dioxide to the above ranges, which can further improve its anti-settling properties and other properties.

[0023] In the present invention, the silane coupling agent in the silane coupling agent modified silica preferably includes one or more of anilinosilane, alkylsilane, epoxysilane and vinylsilane, and more preferably anilinosilane. The present invention selects spherical silica with small particle size, and adopts a silane coupling agent to modify the silica. One end of the silane coupling agent reacts with the hydroxyl group on the surface of the silica, and the other end has good compatibility with the polymer, thereby improving the sedimentation problem of silica, and avoiding sedimentation during placement after being added to the epoxy potting glue. The present invention limits the type of silane coupling agent within the above range, which can further improve its anti-sedimentation property, so that the silica composite slurry has a small thixotropy, low viscosity and high fluidity.

[0024] The raw materials for preparing the silicon dioxide composite slurry of the present invention also include silazane.

[0025] In the present invention, the silazane preferably includes one or both of hexamethyldisilazane and tetramethyldisilazane.

[0026] In the present invention, the mass ratio of the silazane to the silane coupling agent modified silica is (0.1-0.5):100, preferably (0.2-0.5):100, and more preferably (0.3-0.5):100. In the present invention, the silazane can react with the hydroxyl groups on the surface of silica to reduce the hydroxyl content on the surface of silica, thereby improving its thixotropy.

[0027] The present invention limits the type and amount of silazane to the above range, which can further improve its anti-settling property, so that the silica composite slurry has small thixotropy, low viscosity and high fluidity.

[0028] The raw materials for preparing the silicon dioxide composite slurry of the present invention also include acid anhydride.

[0029] In the present invention, the acid anhydride preferably includes one or both of methyltetrahydrophthalic anhydride and methylhexahydrophthalic anhydride. In the present invention, the acid anhydride can be used as a curing agent.

[0030] In the present invention, the mass ratio of the acid anhydride to the silane coupling agent modified silica is (3-8): (3-8), preferably (0.5-1.5): 1. The present invention limits the mass ratio of the acid anhydride to the silane coupling agent modified silica to the above range, which can further improve its anti-settling property, so that the silica composite slurry has small thixotropy, low viscosity and high fluidity.

[0031] The raw materials for preparing the silicon dioxide composite slurry of the present invention also include a accelerator.

[0032] In the present invention, the accelerator preferably includes one or more of a tertiary amine accelerator and an imidazole accelerator. In the present invention, the tertiary amine accelerator preferably includes TAP, DMP-30, BDMA or DETDA; the imidazole accelerator preferably includes 2E4MZ.

[0033] In the present invention, the mass ratio of the accelerator to the acid anhydride is (0.2-2.0):100, preferably (0.5-2.0):100. In the present invention, the accelerator can accelerate the reaction of the curing agent and the epoxy resin in the epoxy potting adhesive. The present invention limits the mass ratio of the accelerator to the acid anhydride within the above range, and when the silica composite slurry is added to the epoxy potting adhesive for use, the reaction speed of the component A and the component B can be moderate.

[0034] In the present invention, the D50 of the silica composite slurry is preferably 0.1 to 2.0 μm; the D100 of the silica composite slurry is preferably ≤8.0 μm; the solid content of the silica composite slurry is preferably 30 to 75%. The present invention limits the particle size and solid content of the silica composite slurry within the above range, which can further make the silica composite slurry have small thixotropy, low viscosity and high fluidity, and improve the anti-settling property of the silica composite slurry.

[0035] The present invention also provides a method for preparing the silicon dioxide composite slurry described in the above technical solution, comprising the following steps:

[0036] (1) performing a first modification on silicon dioxide using a silane coupling agent to obtain silicon dioxide modified with a silane coupling agent;

[0037] (2) The silane coupling agent-modified silica obtained in step (1) is mixed with silazane, anhydride and a promoter, and then subjected to a second modification to obtain a silica composite slurry.

[0038] The present invention uses a silane coupling agent to perform a first modification on silicon dioxide to obtain silane coupling agent-modified silicon dioxide.

[0039] In the present invention, the mass ratio of the silane coupling agent to the silica is preferably (0.2-2): 100, more preferably (0.5-1.5): 100. The present invention limits the mass ratio of the silane coupling agent to the silica to the above range, which can further reduce the thixotropy of the silica composite slurry, have low viscosity and high fluidity, and improve the anti-settling property of the silica composite slurry.

[0040] In the present invention, the temperature of the first modification is preferably 80-150°C, more preferably 110-130°C; the time of the first modification is preferably 20-60min, more preferably 30-50min; the first modification is preferably carried out under stirring conditions; the stirring rate is preferably 500-1500rpm. In the present invention, during the first modification process, the silane coupling agent reacts with the hydroxyl groups on the surface of the silica to generate silane coupling agent-modified silica. The present invention limits the temperature, time and rate of the first modification within the above range, so that the two can react fully.

[0041] After the first modification is completed, the present invention preferably cools the product of the first modification to obtain silane coupling agent-modified silica.

[0042] The present invention has no special limitation on the cooling operation, and cooling to room temperature may be performed using cooling technical solutions well known to those skilled in the art.

[0043] After obtaining the silane coupling agent modified silica, the present invention mixes the silane coupling agent modified silica with silazane, acid anhydride and accelerator and then performs a second modification to obtain a silica composite slurry.

[0044] The present invention has no special limitation on the mixing operation of the silane coupling agent-modified silica with silazane, acid anhydride and accelerator, and the technical scheme of material mixing well known to those skilled in the art can be adopted.

[0045] In the present invention, the temperature of the second modification is preferably 50-90°C, more preferably 60-80°C; the time of the second modification is preferably 20-60 min; the second modification is preferably carried out in a sand mill; the speed of the sand mill is preferably 1000-2000 rpm, more preferably 1500 rpm. In the present invention, during the second modification process, silazane reacts with the hydroxyl groups on the surface of silica in the silane coupling agent-modified silica, and the anhydride and the accelerator are present in the composite slurry in the form of a physical mixture. The present invention limits the temperature and time of the second modification within the above range, so that silazane can fully react with the silane coupling agent-modified silica.

[0046] After the second modification is completed, the present invention preferably cools and filters the product of the second modification in sequence to obtain a silicon dioxide composite slurry.

[0047] The present invention has no special limitation on the cooling operation, and cooling to room temperature may be performed using cooling technical solutions well known to those skilled in the art.

[0048] The present invention has no special limitation on the filtering operation, and a filtering technical solution well known to those skilled in the art can be used to ensure that the particle size of the silica composite slurry is within a limited range.

[0049] The present invention controls various parameters in the preparation process, so that various raw materials can fully react, further making the silicon dioxide composite slurry have small thixotropy, low viscosity and high fluidity, and improving the anti-settling property of the silicon dioxide composite slurry.

[0050] The present invention also provides the use of the silicon dioxide composite slurry described in the above technical solution or the silicon dioxide composite slurry prepared according to the preparation method described in the above technical solution in epoxy potting glue.

[0051] In the present invention, the epoxy potting adhesive preferably includes component A and component B.

[0052] The epoxy potting adhesive provided by the present invention preferably includes component A.

[0053] In the present invention, the A component preferably includes epoxy resin and silica.

[0054] The present invention has no particular limitation on the type and source of the epoxy resin, and any epoxy resin for potting glue well known to those skilled in the art can be used.

[0055] In the present invention, the particle size of the silicon dioxide in the A component is preferably D50=10.0-35.0 μm, D100≤200 μm, and the specific surface area is preferably ≤3.0 m 2 / g.

[0056] The epoxy potting adhesive provided by the present invention preferably also includes a B component.

[0057] In the present invention, the B component preferably includes anhydride, silica and an accelerator.

[0058] The present invention has no special limitation on the type and source of the acid anhydride, and the acid anhydride for epoxy potting adhesive known to those skilled in the art can be used. In the application example of the present invention, the acid anhydride is preferably methyl hexahydrophthalic anhydride.

[0059] The present invention has no special limitation on the type and source of the accelerator, and any accelerator for epoxy potting adhesive known to those skilled in the art can be used. In the application example of the present invention, the accelerator is preferably DMP-30.

[0060] In the present invention, the silicon dioxide in the B component is preferably spherical silicon dioxide; the particle size of the silicon dioxide is preferably D50=10.0-35.0 μm, D100≤200 μm, and the specific surface area is preferably ≤2.0 m 2 / g.

[0061] The silicon dioxide composite slurry provided by the present invention can be used as component B, or can be added to component B to replace part of component B, so as to improve the sedimentation property of component B.

[0062] The epoxy potting adhesive provided by the present invention is divided into A and B components, which are stored separately. When used, the A and B components are mixed before use. After the silicon dioxide composite slurry is used as the B component or added to the B component, the B component will not settle during storage, and has low viscosity, good fluidity and small thixotropy.

[0063] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0064] Example 1

[0065] A silicon dioxide composite slurry is prepared from silicon dioxide modified by a silane coupling agent, silazane, anhydride and a accelerator;

[0066] The preparation method of the silicon dioxide composite slurry is:

[0067] (1) 3 kg of spherical silica (D50 = 0.81 μm, D100 = 3.51 μm, specific surface area SSA = 3.5 m 2 / g) was put into a 10L high-speed stirrer, stirring was started at a speed of 1000 rpm, alkyl silane KBM-13 (Shin-Etsu Chemical, Japan) was added for modification (the mass ratio of alkyl silane to silica was 0.5:100), the modification temperature was 80°C, the modification time was 30 min, and silane coupling agent modified silica was obtained;

[0068] (2) After mixing 2.8 kg of the silane coupling agent modified silica in step (1) with 1.2 kg of methylhexahydrophthalic anhydride, 5.6 g of hexamethyldisilazane and 20 g of DMP-30 (the mass ratio of methylhexahydrophthalic anhydride to the silane coupling agent modified silica is 0.43:1, the mass ratio of hexamethyldisilazane to the silane coupling agent modified silica is 0.2:100, and the mass ratio of DMP-30 to methylhexahydrophthalic anhydride is 1.67:100), a 3L sand mill is used for modification, the rotation speed is 1500 rpm, the modification time is 20 min, the modification temperature is 60 ° C, and the silica composite slurry is obtained by filtering through a filter element filter.

[0069] The D50 and D100 of the silicon dioxide composite slurry in Example 1 were tested using an American Beckman Coulter LS13320 laser particle size analyzer, and the test dispersion medium was MEK.

[0070] The D50 of the silica composite slurry prepared in Example 1 is 0.81 μm, the D100 of the silica composite slurry is 3.51 μm, and the solid content is 70.0%.

[0071] Example 2

[0072] A silicon dioxide composite slurry is prepared from silicon dioxide modified by a silane coupling agent, silazane, anhydride and a accelerator;

[0073] The preparation method of the silicon dioxide composite slurry is:

[0074] (1) 2.5 kg of spherical silica (D50 = 0.51 μm, D100 = 2.66 μm, specific surface area SSA = 6.1 m 2 / g) was put into a 10L high-speed stirrer, stirring was started, and aniline silane KBM-573 (Shin-Etsu Chemical, Japan) was added for modification (the mass ratio of aniline silane to silica was 1:100), the modification temperature was 150°C, the modification time was 50min, and silane coupling agent modified silica was obtained;

[0075] (2) 2.4 kg of the silane coupling agent modified silica in step (1) was mixed with 1.6 kg of methyltetrahydrophthalic anhydride, 6 g of hexamethyldisilazane and 10 g of 2E4MZ (the mass ratio of methyltetrahydrophthalic anhydride to the silane coupling agent modified silica was 0.67:1, the mass ratio of hexamethyldisilazane to the silane coupling agent modified silica was 0.25:100, and the mass ratio of 2E4MZ to methyltetrahydrophthalic anhydride was 0.625:100), and then modified using a 3L sand mill at a rotation speed of 1500 rpm, a modification time of 30 min, and a modification temperature of 80° C. The mixture was filtered through a filter cartridge to obtain a silica composite slurry.

[0076] Using the same test method, the D50 of the silica composite slurry prepared in Example 2 was 0.51 μm, the D100 of the silica composite slurry was 2.66 μm, and the solid content was 60.0%.

[0077] Example 3

[0078] A silicon dioxide composite slurry is prepared from silicon dioxide modified by a silane coupling agent, silazane, anhydride and a accelerator;

[0079] The preparation method of the silicon dioxide composite slurry is:

[0080] (1) 2 kg of spherical silica (D50 = 0.32 μm, D100 = 0.96 μm, specific surface area SSA = 12.5 m 2 / g) was put into a 10L high-speed stirrer, stirring was started, and vinyl silane KBM-1003 (Shin-Etsu Chemical, Japan) was added for modification (the mass ratio of vinyl silane to silicon dioxide was 1.5:100), the modification temperature was 100°C, and the modification time was 50min to obtain silane coupling agent modified silicon dioxide;

[0081] (2) 1.2 kg of the silane coupling agent modified silica in step (1) was mixed with 1.8 kg of methyltetrahydrophthalic anhydride, 6 g of hexamethyldisilazane and 10 g of BDMA (the mass ratio of methyltetrahydrophthalic anhydride to the silane coupling agent modified silica was 1.5:1, the mass ratio of hexamethyldisilazane to the silane coupling agent modified silica was 0.5:100, and the mass ratio of BDMA to methyltetrahydrophthalic anhydride was 0.56:100), and then modified using a 3L sand mill at a rotation speed of 1500 rpm, a modification time of 30 min, and a modification temperature of 80°C, and filtered through a filter cartridge filter to obtain a silica composite slurry.

[0082] Using the same test method, the D50 of the silica composite slurry prepared in Example 3 was 0.33 μm, the D100 of the silica composite slurry was 0.96 μm, and the solid content was 40.0%.

[0083] Example 4

[0084] The alkylsilane in step (1) of Example 1 was replaced by aniline silane KBM-573, and the other parameters were the same as those of Example 1.

[0085] Example 5

[0086] The alkylsilane in step (1) of Example 1 was replaced by epoxysilane KBM-403, and the other parameters were the same as those of Example 1.

[0087] Comparative Example 1

[0088] The silica in step (1) of Example 1 was replaced with a silica having a D50 of 4.2 μm, a D100 of 9.6 μm, and a specific surface area SSA of 1.8 m 2 / g of spherical silica, and other parameters are the same as those in Example 1.

[0089] Comparative Example 2

[0090] Step (1) in Example 1 is omitted, and the other steps are the same as those in Example 1.

[0091] Comparative Example 3

[0092] The hexamethyldisilazide in step (2) of Example 1 was omitted, and other parameters were the same as those in Example 1.

[0093] Comparative Example 4

[0094] The modification temperature in step (2) of Example 1 was replaced with 15° C., and the other parameters were the same as those of Example 1.

[0095] The viscosity, thixotropy, and sedimentation stability (layer height, observe the bottom sediment) of the silica composite slurry in Examples 1 to 5 and Comparative Examples 1 to 4 were tested. The results are shown in Table 1, where sedimentation stability: the slurry was poured into a 100 ml test tube to the 100 ml mark, sealed and placed in a drying oven at 60°C for 7 days to observe the layering of the slurry, record the height of the layered clear liquid, and observe whether there is sedimentation at the bottom after inversion for 5 minutes. The less the layering, the less the bottom sedimentation, and the better the product stability. Viscosity: Using Anton Paar rheometer MCR302e, at 25°C, variable shear mode, the corresponding viscosity when the shear rate is 50 [1 / s]. Thixotropy: Using Anton Paar rheometer MCR 302e, at 25°C, variable shear mode, the ratio of the viscosity corresponding to the shear rate of 5 [1 / s] to the viscosity corresponding to the shear rate of 50 [1 / s], the larger the number, the stronger the thixotropy.

[0096] Table 1 Viscosity, thixotropy, layer height and bottom sedimentation of silica composite slurry in Examples 1 to 5 and Comparative Examples 1 to 4

[0097] name Viscosity, cp Thixotropy Layer height, mm Bottom sediment situation Example 1 821 1.29 0 No sediment Example 2 652 1.35 0 No sediment Example 3 564 1.36 0 No sediment Example 4 712 1.38 0 No sediment Example 5 881 1.40 0 No sediment Comparative Example 1 324 1.35 5 There is sediment Comparative Example 2 1462 2.81 0 No sediment Comparative Example 3 987 3.10 0 No sediment Comparative Example 4 910 2.42 0 No sediment

[0098] It can be seen from Examples 1 to 5 that the viscosities of the examples are different, and the thixotropy is not large; the sedimentation layer height is 0, and there is no sediment, which indicates that the sedimentation stability is good.

[0099] Compared with Example 1, the raw materials are different. The particle size of Example 1 is large, the SSA is small, and the product viscosity is low. The thixotropy is not much different, but the sedimentation layer height is high and there is sediment at the bottom, indicating that the raw materials affect the sedimentation stability.

[0100] Compared with Example 1, Comparative Example 2 does not involve the modification of the silane coupling agent in step (1), but the product has high viscosity and high thixotropy, indicating that the modification of the silane coupling agent in step 1 affects the viscosity and thixotropy.

[0101] Compared with Example 1, in Comparative Example 3, hexamethyldisilazane was not added in step (2), but the product had a slightly higher viscosity and a higher thixotropy, indicating that the hexamethyldisilazane in step (2) would affect the viscosity and thixotropy.

[0102] Compared with Example 1, in Comparative Example 4, the modification temperature in step (2) is low, while the product viscosity and thixotropy are slightly larger, indicating that the modification temperature in step (2) affects the viscosity and thixotropy.

[0103] Application Example 1

[0104] The silica composite slurry prepared in Example 1 was added to the B component of the two-component epoxy potting glue, wherein the B component consisted of a curing agent, methyl hexahydrophthalic anhydride, an accelerator, DMP-30, a D50 of 20.0 μm, a D100 of 48.6 μm, and a specific surface area of ​​0.6 m 2 / g of spherical silica (NQ1160 produced by Jiangsu Lianrui New Materials Co., Ltd.), the mass ratio of curing agent, accelerator and spherical silica is 29.7:0.3:70.0, and the mass ratio of silica composite slurry to component B is 15:100.

[0105] Comparative application example 1:

[0106] Component B in Example 1 was used.

[0107] Comparative Application Example 2

[0108] The silica composite slurry in Application Example 1 was replaced with the anti-settling agent fumed silica AEROSIL200 (Evonik, Germany), and the mass ratio of fumed silica AEROSIL200 to component B was 2:100.

[0109] Comparative Application Example 3

[0110] The silica composite slurry in Application Example 1 was replaced with an organic anti-settling agent BYK-401 (BYK Chemical, Germany), and the mass ratio of BYK-401 to component B was 1:100.

[0111] The viscosity, thixotropy, layer height and bottom sedimentation of component B after adding silica composite slurry, fumed silica AEROSIL200 and organic anti-settling agent BYK-401 to application example 1 and comparative application examples 1 to 3 were tested. The results are shown in Table 2.

[0112] Table 2 shows the viscosity, thixotropy, layer height and bottom sedimentation of component B after adding silica composite slurry in Application Example 1, component B alone in Comparative Application Examples 1 to 3, and adding fumed silica AEROSIL 200 and organic anti-settling agent BYK-401.

[0113]

[0114]

[0115] It can be seen from Table 2 that Example 1, fumed silica AEROSIL 200, and organic anti-settling agent BYK-401 all have good sedimentation stability, but AEROSIL 200 and BYK-401 increase the viscosity and thixotropy of the product, while the product of the present invention has lower viscosity and thixotropy.

[0116] In summary, the silica composite slurry provided by the present invention has excellent anti-settling properties after being added to the epoxy potting adhesive, and has low viscosity and thixotropy.

[0117] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements without departing from the principle of the present invention, and these improvements should also be regarded as within the protection scope of the present invention.

Claims

1. A silica composite slurry, comprising the following raw materials: silane coupling agent modified silica, silazane, acid anhydride and accelerator; the mass ratio of the silazane to the silane coupling agent modified silica is (0.1-0.5):100; the mass ratio of the acid anhydride to the silane coupling agent modified silica is (3-8):(3-8); the mass ratio of the accelerator to the acid anhydride is (0.2-2.0):100; the silane coupling agent modified silica is spherical; the D50 of the silica is 0.1-2.0 μm; the D100 of the silica is ≤8.0 μm; the specific surface area of ​​the silica is 3.0-20 m 2 / g.

2. The silicon dioxide composite slurry according to claim 1, characterized in that The silane coupling agent in the silane coupling agent-modified silica includes one or more of anilinosilane, alkylsilane, epoxysilane and vinylsilane.

3. The silicon dioxide composite slurry according to claim 1, characterized in that: The silazane includes one or both of hexamethyldisilazane and tetramethyldisilazane.

4. The silicon dioxide composite slurry according to claim 1, characterized in that The acid anhydride includes one or both of methyltetrahydrophthalic anhydride and methylhexahydrophthalic anhydride.

5. The silicon dioxide composite slurry according to claim 1, characterized in that: The accelerator includes one or more of a tertiary amine accelerator and an imidazole accelerator.

6. The method for preparing the silicon dioxide composite slurry according to any one of claims 1 to 5, comprising the following steps: (1) performing a first modification on silicon dioxide using a silane coupling agent to obtain silicon dioxide modified with a silane coupling agent; (2) The silane coupling agent-modified silica obtained in step (1) is mixed with silazane, anhydride and a promoter, and then subjected to a second modification to obtain a silica composite slurry.

7. The preparation method according to claim 6, characterized in that: In the step (1), the mass ratio of the silane coupling agent to silicon dioxide is (0.2-2):

100.

8. The preparation method according to claim 6, characterized in that: The temperature of the first modification in step (1) is 80 to 150° C., and the time of the first modification is 20 to 60 minutes.

9. The preparation method according to claim 6, characterized in that: The temperature of the second modification in step (2) is 50 to 90° C., and the time of the second modification is 20 to 60 minutes.

10. Use of the silicon dioxide composite slurry according to any one of claims 1 to 5 or the silicon dioxide composite slurry prepared by the preparation method according to any one of claims 6 to 9 in epoxy potting adhesive.