Application of acid-based deep eutectic solvent in leaching valuable metal from waste ternary lithium battery positive electrode material
Through the acid-based deep eutectic solvent system, the energy consumption and environmental problems of valuable metal recovery in the positive electrode materials of waste lithium battery are solved through the combination of formic acid, dimethylamine hydrochloride and water, and the energy consumption and environmental problems of valuable metal recovery in waste lithium battery are achieved, achieving efficient leaching under mild conditions .
Patent Information
- Application Number
- CN202410973012.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art methods for recycling valuable metals in waste lithium battery positive electrode materials have problems such as large energy consumption, complex operation, equipment corrosion and environmental hazards. The deep eutectic solvent has high viscosity and weak coordination ability, making it difficult to be under mild conditions. Efficiently leaching of valuable metals under the leaching of the valentine.
The acid-based deep eutectic solvent system is used, consisting of formic acid, dimethylamine hydrochloride and water. It is adjusted by the molar ratio of hydrogen bond donor and acceptor to form a stable solvent system, which is efficiently leaching lithium, nickel, and under low temperature water bath conditions. Cobalt and manganese use water diluents to reduce viscosity and promote the diffusion and dissolution of metal ions.
It realizes efficient leaching of valuable metals in the cathode material of waste lithium battery at lower temperatures and short time, reducing energy consumption and environmental impact, and has high economic costs and environmental benefits.
Smart Images

Figure CN118932177A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of waste lithium battery recycling, and specifically relates to the application of an acid-based deep eutectic solvent in leaching valuable metals from anode materials of waste ternary lithium batteries. Background Art
[0002] Lithium-ion batteries are widely used in new energy vehicles, smart electronic devices and other industries due to their high energy density, low self-discharge rate and high operating voltage. After a long period of cyclic use, as the capacity decreases, lithium batteries enter the scrap stage. Waste lithium batteries contain valuable metals such as lithium, nickel, cobalt, manganese, aluminum, and copper, and are mainly concentrated in the positive electrode materials, with high recycling value. In addition, improperly disposed waste lithium batteries are prone to cause serious heavy metal pollution and organic pollution, which is very harmful to the environment. Therefore, there is an urgent need for green and environmentally friendly methods to recover valuable metals from waste lithium batteries.
[0003] Commonly used recycling technologies for waste lithium battery positive electrode materials mainly include pyrometallurgy and hydrometallurgy. Pyrometallurgy mainly uses high-temperature smelting to convert valuable metals in waste lithium battery positive electrode materials into alloys for recycling. However, this method does not achieve the separation of valuable metals in positive electrode materials and has poor applicability.
[0004] At present, there have been many studies that combine pyrometallurgical technology with hydrometallurgical technology. This technology first uses different roasting methods to treat the positive electrode materials of waste lithium batteries, reducing the high-valent transition metal ions in the positive electrode materials to low-valent metal salts, and then uses subsequent hydrometallurgical technology to recover valuable metals. Common roasting methods include sulfidation roasting, chlorination roasting, reduction roasting, etc. The fire-wet combined technology can achieve the selective separation and recovery of lithium and transition metal ions in the positive electrode materials of waste lithium batteries by adjusting the roasting method. However, the fire-wet combined technology is complicated to operate and needs to go through two stages of roasting and leaching. The roasting process often needs to be carried out at high temperatures, so this method consumes a lot of energy.
[0005] Hydrometallurgical technology is mainly divided into inorganic acid leaching and organic acid leaching. Inorganic acid leaching refers to the use of strong acids such as sulfuric acid, hydrochloric acid, and nitric acid to leach the positive electrode materials of waste lithium batteries. Although it can achieve efficient leaching in a short time, inorganic acids are easy to corrode equipment due to their strong acidity and are more harmful to the environment. Organic acid leaching uses organic acids such as citric acid, ascorbic acid, formic acid, and oxalic acid to leach valuable metals in the positive electrode materials of waste lithium batteries. Compared with inorganic acids, organic acids are milder, less toxic, less prone to corroding equipment, and have better environmental benefits. However, due to the low acidity of organic acids, their leaching rate is slow and the consumption time is long.
[0006] Deep eutectic solvents have been widely used in the field of valuable metal recovery in lithium battery cathode materials in recent years. However, the deep eutectic solvent systems currently developed generally have the disadvantages of high viscosity, weak coordination ability, and poor reducibility. They often require higher reaction temperatures and longer leaching times to achieve the leaching of valuable metal ions from waste lithium battery cathode materials. Therefore, there is an urgent need for a green, environmentally friendly method that can leach valuable metals from waste lithium battery cathode materials under relatively mild reaction conditions. Summary of the invention
[0007] In order to solve the deficiencies of the prior art, the present invention aims to provide an acid-based deep eutectic solvent (DES) for recycling spent LiNi x Co y Mn 1-x-y The method of leaching valuable metals in SNCM (O2, SNCM) can efficiently leach lithium, nickel, cobalt and manganese in a short time at a lower temperature, thereby realizing the recovery of valuable metals in SNCM positive electrode materials.
[0008] To achieve the above object, the present invention adopts the following technical solutions:
[0009] (1) Pretreatment of SNCM positive electrode materials: First, the positive electrode materials were immersed in a 20wt% NaCl solution for 24h to fully discharge them. The discharged lithium battery was disassembled and the positive electrode plates were separated. The positive electrode plates were then calcined in a muffle furnace at 500°C for 45min to remove the polyvinylidene fluoride binder in the plates, so that the positive electrode materials were separated from the aluminum foil to obtain SNCM positive electrode material powder.
[0010] (2) Preparation of DES system: A hydrogen bond donor and a hydrogen bond acceptor are added into a glass bottle at a molar ratio of 7 to 10:1, and then a diluent is added. The mixture is heated and stirred in a water bath until the solution becomes clear and transparent to obtain a DES solvent.
[0011] Among them, the hydrogen bond donor is formic acid, and the hydrogen bond acceptor is dimethylamine hydrochloride.
[0012] The diluent is water, and the added amount thereof is 15wt% to 45wt% of the total mass of the hydrogen bond donor and the hydrogen bond acceptor.
[0013] The water bath heating temperature is 60℃~90℃, and the water bath heating time is 2h~5h
[0014] (3) Leaching of valuable metal ions: The pretreated SNCM cathode material powder is mixed with DES at a solid-liquid ratio of 10 g / L to 30 g / L, and then the mixture is heated and stirred in a water bath at a temperature of 60°C to 90°C, a heating time of 2 h to 5 h, and a stirring speed of 400 rpm to achieve the leaching of lithium, nickel, cobalt, and manganese. After the leaching is completed, the leachate is passed through a 0.22 μm hydrophilic PTFE filter membrane to obtain a leachate rich in lithium, nickel, cobalt, and manganese. The concentration of metal ions in the filtrate is measured by an atomic absorption spectrometer, and the leaching rate η of each metal ion is calculated using formula (1).
[0015]
[0016] Where: c is the concentration of lithium, nickel, cobalt and manganese in the leachate, mg / L. V is the volume of the leachate, mL. m is the mass of the added SNCM positive electrode material powder, g. W0 is the mass fraction of lithium, nickel, cobalt and manganese in the original SNCM positive electrode material powder, wt%.
[0017] The present invention forms a stable DES system by mixing formic acid, dimethylamine hydrochloride and water in a certain ratio under stirring conditions in a low-temperature water bath. Both formic acid and dimethylamine hydrochloride in the DES system have certain reducing properties, which can reduce the high-valent transition metal ions in SNCM to divalent metal ions. At the same time, H + It can destroy the ionic bond formed between metal and oxygen and promote the leaching of metal ions. In addition, the Cl provided by dimethylamine hydrochloride as a hydrogen bond acceptor - It can form a complex with the reduced divalent transition metal ions. This reaction accelerates the dissolution of SNCM in the deep eutectic solvent. Water added as a diluent in DES can reduce the viscosity of the system, facilitate the diffusion of substances in the leaching process, and reduce the temperature and time required for the leaching reaction. Therefore, DES prepared with dimethylamine hydrochloride, formic acid and water can efficiently leach valuable metals in SNCM at a lower temperature and in less time.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] (1) The acid-based deep eutectic solvent designed by the present invention has certain acidity and reducing properties, low viscosity, and strong coordination ability, and can quickly and efficiently leach valuable metals in SNCM.
[0020] (2) The deep eutectic solvent designed by the present invention is prepared from formic acid, dimethylammonium hydrochloride and water, and does not involve the use of strong acids, strong bases and reducing agents, thus having lower economic costs and higher environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0022] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0023] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0024] Example 1
[0025] First, the waste lithium battery was immersed in a 20wt% NaCl solution for 24h to fully discharge it. The discharged lithium battery was disassembled and the positive electrode was separated. The positive electrode was then calcined in a muffle furnace at 500℃ for 45min to remove the polyvinylidene fluoride binder in the electrode, so that the positive electrode material was separated from the aluminum foil to obtain SNCM positive electrode material powder.
[0026] Formic acid and dimethylamine hydrochloride were mixed evenly in a molar ratio of 8:1, and then 30 wt % of water was added. The mixture was heated and stirred in a water bath at 60° C. for 30 min to form a light yellow transparent solution, indicating that the preparation of DES was completed.
[0027] The pretreated SNCM cathode material powder and DES were then added to a small glass bottle at a solid-liquid ratio of 20 g / L and heated and stirred for 3 h in a water bath at 80 °C. The leached solution was then filtered through a 0.22 μm hydrophilic PTFE filter membrane, and the concentrations of lithium, nickel, cobalt, and manganese in the filtrate were determined using an atomic absorption spectrometer, and the leaching rate of each metal element was calculated.
[0028] Example 2
[0029] The difference between this embodiment and embodiment 1 is that in the preparation process of DES, the molar ratio of formic acid to dimethylamine hydrochloride is 7:1, and the rest of the preparation process and leaching process are the same as those of embodiment 1. The concentrations of lithium, nickel, cobalt and manganese in the filtrate are determined by atomic absorption spectrometer and the leaching rate of each metal element is calculated.
[0030] Example 3
[0031] The difference between this embodiment and embodiment 1 is that in the preparation process of DES, the molar ratio of formic acid to dimethylamine hydrochloride is 9:1, and the rest of the preparation process and leaching process are the same as those of embodiment 1. The concentrations of lithium, nickel, cobalt and manganese in the filtrate are determined by atomic absorption spectrometer and the leaching rate of each metal element is calculated.
[0032] Example 4
[0033] The difference between this embodiment and embodiment 1 is that in the preparation process of DES, the molar ratio of formic acid to dimethylamine hydrochloride is 10:1, and the rest of the preparation process and leaching process are the same as those of embodiment 1. The concentrations of lithium, nickel, cobalt and manganese in the filtrate are determined by atomic absorption spectrometer and the leaching rate of each metal element is calculated.
[0034] Comparative Example 1
[0035] The difference between this comparative example and Example 1 is that formic acid as a hydrogen bond donor is used to directly leach the SNCM positive electrode material powder, and the rest of the process is the same as Example 1. The concentrations of lithium, nickel, cobalt, and manganese in the filtrate are measured by atomic absorption spectrometer and the leaching rate of each metal element is calculated.
[0036] Comparative Example 2
[0037] The difference between this comparative example and Example 1 is that hydroxylamine hydrochloride is used as a hydrogen bond donor to synthesize DES to leach SNCM positive electrode material powder, and the rest of the process is the same as Example 1. The concentrations of lithium, nickel, cobalt, and manganese in the filtrate are determined by atomic absorption spectrometry and the leaching rate of each metal element is calculated. That is, formic acid and hydroxylamine hydrochloride are mixed evenly in a molar ratio of 8:1, and then 30wt% of water is added, and heated and stirred for 30min in a water bath at 60°C to form a light yellow transparent solution to prepare DES.
[0038] Comparative Example 3
[0039] The difference between this comparative example and Example 1 is that betaine hydrochloride is used as a hydrogen bond donor to synthesize DES to leach SNCM positive electrode material powder, and the rest of the process is the same as Example 1. The concentrations of lithium, nickel, cobalt, and manganese in the filtrate are determined by atomic absorption spectrometry and the leaching rate of each metal element is calculated. That is, formic acid and betaine hydrochloride are mixed evenly in a molar ratio of 8:1, and then 30wt% of water is added, and heated and stirred for 30min in a water bath at 60°C to form a light yellow transparent solution to prepare DES.
[0040] The leaching rates of lithium, nickel, cobalt and manganese in the above examples and comparative examples were calculated and compared with those in Example 1, and the results are shown in Table 1.
[0041] Table 1 Effect of different molar ratios of formic acid and betaine hydrochloride on the leaching rates of lithium, nickel, cobalt and manganese
[0042]
[0043] It can be seen from Table 1 that when formic acid is directly used to leach the SNCM cathode material, the leaching rate of each metal ion is much lower than the leaching rate using DES as the leaching solvent. The reason may be that formic acid does not have coordination ability and its reducing property is not enough to completely reduce the high-valent transition metal ions in the SNCM cathode material, resulting in a low leaching rate. According to Examples 1 to 4, when the molar ratio of formic acid to dimethylamine hydrochloride is less than 8:1, the H ionized in the DES system + The ion bond between transition metal ions and oxygen ions cannot be quickly and effectively destroyed, resulting in a low leaching rate of metal ions. When the molar ratio of formic acid to dimethylamine hydrochloride is greater than 8:1, the Cl - The content is low, because dimethylamine hydrochloride provides Cl - The ability to coordinate with transition metal ions increases the ability of DES solvent to dissolve SNCM cathode material powder. - When the content is insufficient, the leaching rate of the reaction will be low. Therefore, the molar ratio of formic acid to dimethylamine hydrochloride is selected as 8:1 in the following examples.
[0044] Example 5
[0045] The difference between this embodiment and embodiment 1 is that, in the preparation process of DES, the amount of diluent added is 15wt%, and the rest of the preparation process and leaching process are the same as those of embodiment 1. The concentrations of lithium, nickel, cobalt and manganese in the filtrate are measured by atomic absorption spectrometer and the leaching rate of each metal element is calculated.
[0046] Example 6
[0047] The difference between this embodiment and embodiment 1 is that, in the preparation process of DES, the amount of water added as a diluent is 45wt%, and the rest of the preparation process and leaching process are the same as those of embodiment 1. The concentrations of lithium, nickel, cobalt and manganese in the filtrate are measured by atomic absorption spectrometer and the leaching rate of each metal element is calculated.
[0048] The leaching rates of lithium, nickel, cobalt and manganese in the above examples were calculated and compared with those in Example 1, and the results are shown in Table 2.
[0049] Table 2 Effect of different moisture contents in DES on the leaching rates of lithium, nickel, cobalt and manganese
[0050]
[0051] It can be seen from Table 2 that when the amount of water added is 15wt%, the viscosity of the DES solvent is high, which affects the mass transfer of dissolved substances during the leaching process, resulting in poor leaching effect of metal ions. When the amount of water added reaches 45wt%, the excessively high water content will destroy the structure of the DES solvent and affect the leaching effect of metal ions. Therefore, the amount of water added in the following examples is selected to be 30wt%.
[0052] Example 7
[0053] The difference between this embodiment and embodiment 1 is that the temperature of the water bath during the leaching process is 60° C., and the other reaction conditions and the DES preparation process are exactly the same as those in embodiment 1. The concentrations of lithium, nickel, cobalt and manganese in the filtrate are determined by atomic absorption spectrometer and the leaching rate of each metal element is calculated.
[0054] Example 8
[0055] The difference between this embodiment and embodiment 1 is that the temperature of the water bath during the leaching process is 70° C., and the other reaction conditions and the DES preparation process are exactly the same as those in embodiment 1. The concentrations of lithium, nickel, cobalt and manganese in the filtrate are determined by atomic absorption spectrometer and the leaching rate of each metal element is calculated.
[0056] Example 9
[0057] The difference between this embodiment and embodiment 1 is that the temperature of the water bath during the leaching process is 90° C., and the other reaction conditions and the DES preparation process are exactly the same as those in embodiment 1. The concentrations of lithium, nickel, cobalt and manganese in the filtrate are determined by atomic absorption spectrometer and the leaching rate of each metal element is calculated.
[0058] The leaching rates of lithium, nickel, cobalt and manganese in the above examples were calculated and compared with those in Example 1, and the results are shown in Table 3.
[0059] Table 3 Effect of different leaching temperatures on the leaching rates of lithium, nickel, cobalt and manganese
[0060]
[0061] It can be seen from Table 3 that temperature has a significant effect on the leaching rate of each metal element. As the temperature increases, it is beneficial to enhance the reducing ability of the reaction system, and the viscosity of the reaction system is also lower at a higher temperature, so the increase in temperature has a promoting effect on the leaching of metal ions. It is found through the examples that when the temperature is 80°C, the leaching rate of each metal element exceeds 98%, and when the temperature exceeds 80°C, the reaction tends to equilibrium. Therefore, considering economic factors, the leaching temperature selected in the following examples is 80°C.
[0062] Example 10
[0063] The difference between this embodiment and embodiment 1 is that the water bath heating time during the leaching process is 2 hours, and the other reaction conditions and DES preparation process are exactly the same as those in embodiment 1. The concentrations of lithium, nickel, cobalt and manganese in the filtrate are determined by atomic absorption spectrometer and the leaching rate of each metal element is calculated.
[0064] Embodiment 11
[0065] The difference between this embodiment and embodiment 1 is that the water bath heating time during the leaching process is 4 hours, and the other reaction conditions and DES preparation process are exactly the same as those in embodiment 1. The concentrations of lithium, nickel, cobalt and manganese in the filtrate are determined by atomic absorption spectrometer and the leaching rate of each metal element is calculated.
[0066] Example 12
[0067] The difference between this embodiment and embodiment 1 is that the water bath heating time during the leaching process is 5 hours, and the other reaction conditions and DES preparation process are exactly the same as those in embodiment 1. The concentrations of lithium, nickel, cobalt and manganese in the filtrate are measured by atomic absorption spectrometer and the leaching rate of each metal element is calculated.
[0068] The leaching rates of lithium, nickel, cobalt and manganese in the above examples were calculated and compared with those in Example 1, and the results are shown in Table 4.
[0069] Table 4 Effect of different leaching time on leaching rate of lithium, nickel, cobalt and manganese
[0070]
[0071] Table 4 shows that as the leaching time gradually increases from 1h to 3h, the leaching rate of each metal element gradually increases. When the leaching time is short, it is not enough to completely leach the valuable metals in SNCM. As the leaching time continues to increase, the leaching rate tends to balance, indicating that the leaching reaction of the SNCM positive electrode material powder has reached equilibrium. Therefore, considering economic factors comprehensively, the leaching time selected in the following examples is 3h.
[0072] Example 13
[0073] The difference between this embodiment and embodiment 1 is that the solid-liquid ratio of SNCM positive electrode material powder to DES solvent is 10 g / L, and the other reaction conditions and DES preparation process are exactly the same as those in embodiment 1. The concentrations of lithium, nickel, cobalt and manganese in the filtrate were determined by atomic absorption spectrometer and the leaching rate of each metal element was calculated.
[0074] Embodiment 14
[0075] The difference between this embodiment and embodiment 1 is that the solid-liquid ratio of SNCM positive electrode material powder to DES solvent is 30 g / L, and the other reaction conditions and DES preparation process are exactly the same as those in embodiment 1. The concentrations of lithium, nickel, cobalt and manganese in the filtrate were determined by atomic absorption spectrometer and the leaching rate of each metal element was calculated.
[0076] The leaching rates of lithium, nickel, cobalt and manganese in the above examples were calculated and compared with those in Example 1, and the results are shown in Table 5.
[0077] Table 5 Effect of different solid-liquid ratios on leaching rates of lithium, nickel, cobalt and manganese
[0078]
[0079] Table 5 reflects the effect of the solid-liquid ratio of SNCM positive electrode material powder and DES solvent on the leaching efficiency. It can be seen that when the solid-liquid ratio is 10g / L and 20g / L, both have good leaching rates. When the solid-liquid ratio reaches 30g / L, the leaching rate decreases. The reason is that too high a solid powder concentration will affect the mass transfer coefficient of the reaction system, resulting in a decrease in the leaching rate of valuable metals. Therefore, after comprehensive consideration, a solid-liquid ratio of 20g / L is selected as the optimal solid-liquid ratio for this method.
[0080] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
Claims
1. An application of an acid-based deep eutectic solvent, characterized in that: The acid-based deep eutectic solvent is used to leach valuable metals in the positive electrode material of waste ternary lithium batteries. The acid-based deep eutectic solvent is obtained by mixing a hydrogen bond donor, a hydrogen bond acceptor and water in proportion.
2. The use of the acid-based deep eutectic solvent according to claim 1, characterized in that: The hydrogen bond donor is formic acid, and the hydrogen bond acceptor is dimethylamine hydrochloride.
3. The use of the acid-based deep eutectic solvent according to claim 1, characterized in that: The molar ratio of the hydrogen bond donor to the hydrogen bond acceptor is 7 to 10:
1.
4. The use of the acid-based deep eutectic solvent according to claim 1, characterized in that: The method steps for leaching valuable metals in the cathode material of waste ternary lithium batteries are as follows: (1) adding a hydrogen bond donor and a hydrogen bond acceptor into a glass bottle according to a molar ratio, and adding a diluent, and then heating the mixed liquid in a water bath until the solution becomes clear and transparent; (2) The pretreated waste ternary lithium battery positive electrode material powder is mixed with the product of step (1) according to the solid-liquid ratio, and then heated and stirred in a water bath, and the leachate is passed through a 0.22 μm hydrophilic PTFE filter membrane to obtain a leachate rich in lithium, nickel, cobalt, and manganese.
5. The use of the acid-based deep eutectic solvent according to claim 4, characterized in that: The diluent described in step (1) is water, and its added amount is 15wt% to 45wt% of the total mass of the hydrogen bond donor and the hydrogen bond acceptor.
6. The use of the acid-based deep eutectic solvent according to claim 4, characterized in that: The water bath heating temperature of the mixture in step (1) is 60° C. to 90° C., and the water bath heating time is 2 h to 5 h.
7. The use of the acid-based deep eutectic solvent according to claim 4, characterized in that: The water bath heating temperature in step (2) is 60° C. to 90° C., the water bath heating time is 2 h to 5 h, and the water bath heating stirring speed is 400 rpm.
8. The use of the acid-based deep eutectic solvent according to claim 4, characterized in that: The solid-to-liquid ratio in step (2) is 10 g / L to 30 g / L.
Citation Information
Cited By
Method for selectively recycling lithium iron phosphate battery and application thereof
CN120319926A