Positive electrode material, preparation method thereof, positive electrode plate and electrochemical device

By introducing appropriate proportions of element A into the high-nickel ternary positive electrode material to form a cavity structure, the problem of stress rupture during charging and discharging is solved, the cycle life and volume energy density of the battery are improved, and better battery performance is achieved.

CN118943352APending Publication Date: 2024-11-12ENVISION DYNAMICS TECH (JIANGSU) CO LTD +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310531853.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The high-nickel ternary cathode material has a microscopic stress rupture during charging and discharging, resulting in the deterioration of the battery's circulation and gas production performance. The existing technology modification methods are complex and cannot meet market demand.

Method used

Design a positive electrode material, which is a secondary particle formed by the aggregation of primary particles, contains a cavity structure inside, and forms a suitable cavity rate to buffer the volume during charging and discharging by introducing an appropriate proportion of A element when the precursor is formed. Strain to avoid secondary particles rupture.

Benefits of technology

The cycle life and volume energy density of the cathode material are improved, stress accumulation is alleviated through the internal cavity structure, and the cycle performance and gas production performance of the battery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943352A_ABST
    Figure CN118943352A_ABST
Patent Text Reader

Abstract

The invention provides a positive electrode material and a preparation method thereof, a positive electrode plate and an electrochemical device, and belongs to the technical field of lithium ion batteries, the positive electrode material is a secondary particle formed by gathering primary particles, and the interior of the secondary particle comprises a cavity structure. According to the positive electrode material and the preparation method thereof, the positive electrode plate and the electrochemical device, based on the positive correlation characteristics of the content of the element A in the particles of the positive electrode material and the cavity rate, a proper proportion of the element A is introduced when the precursor of the positive electrode material is formed, so that a cavity structure formed in the precursor in an accompanying manner is in a proper cavity rate; therefore, the positive electrode material can buffer the volume strain in the charge-discharge process through a cavity structure with a proper proportion in the positive electrode material and alleviate the fracture phenomenon of secondary particles in the cycle process, thereby prolonging the cycle life and improving the volume energy density of the positive battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a positive electrode material and a preparation method thereof, a positive electrode plate and an electrochemical device. Background Art

[0002] High nickel ternary cathode material (LiNi x Co y Mn 1-x-y O2), which is widely used in high specific energy lithium-ion battery systems because of its high theoretical specific capacity (276mAh / g), high voltage platform (3.6V) and high tap density. Among them, high nickel ternary positive electrode materials can further obtain high specific energy and low cost ternary materials by increasing the nickel content in the material and reducing the cobalt content. However, considering that the ternary positive electrode material is a secondary particle ball formed by the accumulation of primary particles, the high nickel ternary positive electrode material LiNi x Co y Mn 1-x-y O2 (x ≥ 0.8, y ≤ 0.1) will produce large micro-stress between primary particles during the charge and discharge process. This micro-stress will gradually accumulate with the cycle, eventually leading to the rupture of secondary particles and the deterioration of the battery's cycle and gas production performance.

[0003] At present, the main means of modifying ternary positive electrode materials in the existing technology is still element doping and coating optimization. Although the above methods can improve the cycle performance of ternary materials to a certain extent, they will make the preparation process of ternary materials more complicated and cumbersome, and cannot meet market demand.

[0004] Therefore, it is necessary to design a positive electrode material and a preparation method thereof, a positive electrode plate and an electrochemical device to solve the above problems. Summary of the invention

[0005] In view of the above shortcomings of the prior art, the present invention provides a positive electrode material and a preparation method thereof, a positive electrode plate and an electrochemical device, which are used to solve the technical problem in the prior art that the positive electrode material is easily fractured due to microscopic stress during the charge and discharge process, resulting in deterioration of the battery's cycle and gas production performance.

[0006] To achieve the above-mentioned object and other related objects, the present invention provides a positive electrode material, wherein the positive electrode material is a secondary particle formed by aggregation of primary particles, and the secondary particle contains a cavity structure.

[0007] In one example of the present invention, the chemical formula of the positive electrode material is Li 1+a [Ni x Co y M z ]O 2-b A b, 0.7≤x<1, 0≤y<0.3, 0≤z<0.3, -0.2<a<0.2, 0≤b<0.2, x+y+z=1; wherein the M element includes one or more of Mn, Al, Ti, Zr, Mg, Sr, W, Mo, B, V, Se, Nb, Ru, Rh, Pd, Sb, Te, Ce, Ca, Zn, Y and W, and the A element includes one or more of F, N, Cl, S and P.

[0008] In an example of the present invention, at least one element of the A elements is attached to the inner layer of the cavity structure.

[0009] In an example of the present invention, the element attached to the inner layer of the cavity structure includes sulfur, and the cavity ratio of the positive electrode material is positively correlated with the content of the sulfur element in the positive electrode material.

[0010] In one example of the present invention, when the sulfur content in the secondary particles is 0.01wt% to 0.35wt%, the positive electrode material has a cavity rate of 0.5% to 10%, and the particle tap density of the positive electrode material is 2.38 to 2.81g / cm 3 .

[0011] In one example of the present invention, the valence state of the sulfur element in the positive electrode material is at least one of -2, +4 or +6; wherein the sulfur element is retained in the cavity structure in the form of at least one of sulfide ions, thiosulfate ions, sulfate ions and sulfite ions.

[0012] In one example of the present invention, when the sulfur content in the secondary particles is 0.01wt% to 0.1wt%, the XPS photoelectron peak binding energy range of the sulfur element in the positive electrode material is 168±2eV; when the sulfur content in the secondary particles is 0.01wt% to 0.05wt%, the XPS photoelectron peak binding energy range of the sulfur element in the positive electrode material is 168.5±1eV.

[0013] In an example of the present invention, the inner diameter of the cavity structure is 10 nm to 1 μm.

[0014] The present invention also provides a method for preparing a positive electrode material, the preparation method comprising:

[0015] A nickel source, a cobalt source, an M element carrier, a precipitant and a complexing agent are mixed for a coprecipitation reaction to obtain a nickel-cobalt precursor material; the nickel-cobalt precursor material is mixed with a lithium source and then sintered to obtain a positive electrode material; wherein the M element includes one or more of Mn, Al, Ti, Zr, Mg, Sr, W, Mo, B, V, Se, Nb, Ru, Rh, Pd, Sb, Te, Ce, Ca, Zn, Y and W, and at least one element carrier among the nickel source, cobalt source and M source is sulfate; during the synthesis process of the coprecipitation reaction, the nickel-cobalt precursor forms a cavity structure inside the secondary particles.

[0016] In one example of the present invention, the nickel source, cobalt source, and M element carrier source include element A, and the element A includes one or more of F, N, Cl, S, and P, wherein during the co-precipitation reaction synthesis process of the nickel-cobalt precursor, the element A is attached to the inside of the cavity structure.

[0017] In an example of the present invention, the sulfur element in the A element is attached to the inside of the cavity structure, and the cavity ratio of the positive electrode material is 0.5% to 10%.

[0018] The present invention also provides a positive electrode plate, which includes a positive electrode current collector and a positive electrode active material layer, and the positive electrode active material layer adopts the positive electrode material described in any of the above examples.

[0019] The present invention also provides an electrochemical device, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet comprises the positive electrode material described in any of the above examples, or the positive electrode material prepared by the preparation method described in any of the above examples.

[0020] The positive electrode material and its preparation method, positive electrode plate and electrochemical device in the present invention are based on the positive correlation between the A element content and the cavity rate in the positive electrode material particles. By introducing an appropriate proportion of the A element when the positive electrode material precursor is formed, the cavity structure formed inside the precursor is at an appropriate cavity rate, so as to ensure that the positive electrode material can buffer the volume strain during the charge and discharge process through the cavity structure with an appropriate proportion inside, and alleviate the rupture phenomenon of secondary particles during the cycle process, thereby improving the cycle life and volume energy density of the positive battery. Therefore, the present invention effectively overcomes some practical problems in the prior art and has high utilization value and use significance. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 This is a scanning electron microscope test image of the positive electrode material in the present invention.

[0023] Figure 2 It is a schematic diagram of the process of preparing the positive electrode material in the present invention.

[0024] Component number description

[0025] 1. Secondary particles; 2. Cavity structure. DETAILED DESCRIPTION

[0026] The following is an explanation of the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the features in the following embodiments and the embodiments can be combined with each other without conflict. It should also be understood that the terms used in the embodiments of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods for which specific conditions are not specified in the following examples are usually carried out under conventional conditions or according to the conditions recommended by the manufacturers.

[0027] It should be noted that the terms such as "upper", "lower", "left", "right", "middle" and "one" etc. used in this specification are only for the convenience of description and are not intended to limit the scope of implementation of the present invention. Changes or adjustments to their relative relationships, without substantially changing the technical content, should also be regarded as the scope of implementation of the present invention.

[0028] The present invention discloses a positive electrode material and a preparation method thereof, a positive electrode plate and an electrochemical device. When a positive electrode material precursor is formed, an appropriate proportion of A element is introduced so that the cavity structure formed inside the precursor has an appropriate cavity ratio, so as to ensure that the positive electrode material can buffer the volume strain during the charge and discharge process through the cavity structure with an appropriate proportion inside, and alleviate the rupture of secondary particles during the cycle process, thereby solving the technical problem in the prior art that the positive electrode material is easily ruptured due to microscopic stress during the charge and discharge process, resulting in deterioration of the cycle and gas production performance of the battery.

[0029] See also Figure 1, the cathode material of the present invention is a high-nickel ternary cathode material. The cathode material is spherical secondary particles 1 formed by the aggregation of primary particles. Discrete cavity structures 2 are contained inside the spherical secondary particles 1. The cavity structures 2 existing inside the secondary particles 1 have rich morphologies. These cavity structures 2 contribute to the release of microscopic stress generated during the charge and discharge process of the cathode material, relieve the cracking of the secondary particles 1 caused by the stress accumulation between the primary particles, and thus improve the cycle life of the cathode material. It should be noted that the cavity structure is a hollow cavity structure formed inside the secondary particles of the cathode material due to the volatilization and gas generation of internal elements during the sintering and forming process. Among them, during the formation process of the cavity structure of the cathode material, element A introduced into the cathode material will adhere to the inner wall of the cavity structure, thereby expanding the volume of the cavity structure.

[0030] Among them, the primary particles of the cathode material are high-nickel ternary materials, and the chemical formula of the high-nickel ternary material is Li 1+a [Ni x Co y M z O 2-b A b ; where 0.7 ≤ x < 1, 0 ≤ y < 0.3, 0 ≤ z < 0.3, -0.2 < a < 0.2, 0 ≤ b < 0.2, and x + y + z = 1. In an optional embodiment, the high-nickel ternary material is preferably Li 1+a [Ni x Co y M z O 2-b A b , where 0.8 ≤ x < 1, 0 ≤ y < 0.1, 0 ≤ z < 0.2, -0.2 < a < 0.2, 0 ≤ b < 0.2, and x + y + z = 1.

[0031] In some embodiments, the M element in the high-nickel ternary material is selected from any one or more of Mn, Al, Ti, Zr, Mg, Sr, W, Mo, B, V, Se, Nb, Ru, Rh, Pd, Sb, Te, Ce, Ca, Zn, Y, and W. That is, the M element can be any one of the above-listed element types, such as Mn, Al, Ti, Zr, Mg, Sr, W, Mo, or B, etc.; the M element can be any combination of two or more of the above-listed element types, such as the combination of Mn and Zr, or the combination of Al and Ti, or the combination of Al and Ce, or the combination of Mn, Al, and W, or the combination of Mn, Al, Nb, and Ru, etc., and will not be listed one by one here.

[0032] The A element in the high nickel ternary material is selected from any one or more of F, N, Cl, S and P. That is, the A element can be any one of the element types listed above, such as F, N, Cl, S or P, etc.; the A element can be any combination of two or more of the element types listed above, for example, the A element is a combination of S and Cl, or a combination of F and S, or a combination of N and Cl, or a combination of S, P and Cl, or a combination of S, N, F and Cl, etc., which are not listed here one by one.

[0033] In addition, when the A element and the M element are two or more combinations, there is no restriction on the ratio of each element in the combination, and they can be mixed in any ratio, etc. In other embodiments, the A element and the M element can also be element types not listed above.

[0034] Among them, the A element contained in the positive electrode material is retained in the secondary particles when the nickel source, cobalt source, and M element carrier are coprecipitated to synthesize the nickel-cobalt precursor. In one embodiment of the present invention, in the positive electrode material, at least one element of the A element is attached to the cavity structure in the secondary particles, and the A element retained in the cavity is positively correlated with the cavity rate in the secondary particles. Therefore, for the positive electrode material, the microstructure inside the secondary particles of the positive electrode material can be judged by the cavity rate of the positive electrode particle cross section and the A element content index. It should be noted that the "cavity rate" of the positive electrode material in this article refers to the area ratio of the cavity structure in the cross section of the secondary particle and the cavity rate can be measured as follows: by cutting the secondary particles of the positive electrode material using a focused ion beam, then taking a cross-sectional photo using a scanning electron microscope, and then using the cross-sectional photo to calculate the ratio of the total area of ​​the cavity structure to the cross-sectional area of ​​the secondary particle. The A element content in the positive electrode material can be obtained by EDS energy spectrum analysis tested by transmission electron microscopy.

[0035] In the positive electrode material, at least one element contained in the A element is attached to the inner wall of the cavity structure in the secondary particles. When the cavity ratio of the secondary particle cross-section and the A element content are in a suitable range, for example, when the cavity ratio is 0.5% to 10%, the cavity structure inside the positive electrode material is rich in morphology. These cavity structures help to release the microscopic stress generated by the positive electrode material during the charging and discharging process, alleviate the secondary particle rupture caused by the stress accumulation between the primary particles, thereby improving the cycle life of the high-nickel positive electrode material.

[0036] When the void ratio and the A element content in the positive electrode material are too low (that is, the void ratio of the positive electrode material is less than 0.5%), the secondary particles of the positive electrode material are relatively dense and have a high tap density. The stress generated by the volume phase change of the material during charging and discharging has nowhere to be released, which can easily lead to secondary particle rupture during stress accumulation, making it difficult to improve the cycle life of the positive electrode material; and when the void ratio and the A element content in the positive electrode material are too high (that is, the void ratio of the positive electrode material is greater than or equal to 15%), the tap density of the positive electrode material particles is low, the volume energy density of the battery cell is low, and the contact area with the electrolyte increases during charging and discharging, which intensifies the side reactions with the electrolyte and worsens the cycle of the positive electrode material.

[0037] It should be noted that the tap density (TD) refers to the volume of the powder when a certain amount of powder is put into a container and vibrated regularly under certain conditions to compress the gaps between the particles as much as possible, and finally to the extent that the gaps between the particles cannot be reduced, and then the weight of the powder is divided by the volume to obtain the tap density. The tap density of the positive electrode material in the present invention is obtained by testing according to the national standard GB / T5162-2006.

[0038] In some embodiments, the element attached to the inner layer of the cavity structure includes sulfur. When the sulfur content in the positive electrode material is 0.01wt% to 0.35wt%, the secondary particle cross section of the positive electrode material has a cavity rate of 0.5% to 10%. At this time, the particle tap density of the positive electrode material is 2.38 to 2.81g / cm 3 The positive electrode material can maintain a capacity retention rate of more than 80% after 800 cycles, has a low gas production growth, and has a long cycle life.

[0039] Preferably, when the sulfur content in the positive electrode material is 0.01wt% to 0.05wt%, the secondary particle cross section of the positive electrode material has a cavity rate of 0.5% to 5%, and the particle tap density of the positive electrode material is 2.49 to 2.81g / cm 3 At this time, the capacity retention rate of the positive electrode material can be maintained at more than 80% after 800 cycles, and the gas production growth is low at different cavity rates within the range. The gas production growth rate of the positive electrode material after working for 56 days is less than 4%.

[0040] In some embodiments, the valence state of the sulfur element in the positive electrode material is at least one of -2, +4 and +6, and the sulfur element in the positive electrode material is retained in the cavity structure in the form of at least one of sulfide ions, thiosulfate ions, sulfate ions and sulfite ions.

[0041] Among them, the content of sulfur element in the secondary particles will affect the valence state of sulfur element in the positive electrode material. For example, when the content of sulfur element in the secondary particles of the positive electrode material is 0.01wt% to 0.1wt%, the XPS photoelectron peak binding energy range of sulfur element in the positive electrode material is 168±2eV, the valence state of sulfur element in the positive electrode material is -2, +4 and +6, and the sulfur element is retained in the cavity structure in the form of sulfide ions, thiosulfate ions, sulfate ions and sulfite ions; when the content of sulfur element in the secondary particles of the positive electrode material is 0.01wt% to 0.05wt%, the XPS photoelectron peak binding energy range of sulfur element in the positive electrode material is 168.5±1eV, the valence state of sulfur element in the positive electrode material is +4 and +6, and the sulfur element is retained in the cavity structure in the form of sulfate ions and sulfite ions.

[0042] like Figure 1 As shown, in some embodiments, the inner diameter of the cavity structure within the secondary particles of the positive electrode material is 10 nm to 1 μm.

[0043] See also Figure 2 The present invention provides a method for preparing a positive electrode material, comprising the following steps:

[0044] S1, mixing a nickel source, a cobalt source and an M element carrier with a precipitant and a complexing agent for coprecipitation reaction, and washing and drying the product after the coprecipitation reaction is completed to obtain a nickel-cobalt precursor material; wherein the nickel-cobalt precursor is Ni x Co y M z (OH) 2-b A b ;

[0045] S2. Mixing the nickel-cobalt precursor material with a lithium source and sintering the mixture, and crushing and classifying the sintered product to obtain a finished positive electrode material.

[0046] Step S1 specifically includes: pumping a nickel source, a cobalt source and an M element carrier into a continuously stirred reactor according to the molar ratio of nickel element, cobalt element and M element (70-100): (0-30): (0-30) to obtain a mixed solution, and then mixing the mixed solution with a precipitant aqueous solution and a complexing agent aqueous solution to perform a coprecipitation reaction and ageing to obtain a solid-liquid mixture; filtering the solid-liquid mixture to obtain a filter cake, washing the filter cake, and drying the filter cake to obtain a nickel-cobalt precursor Ni x Co y M z (OH) 2-b A b, wherein 0.7≤x<1, 0≤y<0.3, 0≤z<0.3, 0≤b<0.2, x+y+z=1, and the molar ratio of each element can be selected within the above range according to specific needs.

[0047] In step S1, the nickel source, the cobalt source and the M element carrier are soluble salts carrying nickel, cobalt and M elements, respectively. As an example, the nickel source, the cobalt source and the M element carrier can be one or more of soluble sulfates, oxalates, acetates, chlorides, nitrates or carbonates. Wherein, the nickel source, the cobalt source and the M element carrier include the A element, and the A element is selected from any one or more of F, N, Cl, S and P, and the M element is selected from any one or more of Mn, Al, Ti, Zr, Mg, Sr, W, Mo, B, V, Se, Nb, Ru, Rh, Pd, Sb, Te, Ce, Ca, Zn, Y and W.

[0048] Preferably, in some embodiments, at least one of the nickel source, cobalt source and M element carrier used in step S1 is sulfate.

[0049] There is no particular limitation on the above solvent, as long as it can dissolve the nickel source, the cobalt source and the M element carrier source. As an example, the solvent can be selected from one or more of deionized water, methanol, ethanol, acetone, isopropanol and n-hexanol.

[0050] The precipitant is selected from one or more of NaOH, KOH and LiOH; the complexing agent is selected from one or more of ammonia water, ammonium bicarbonate, ammonium carbonate, citric acid and ethylenediaminetetraacetic acid.

[0051] Among them, the nickel-cobalt precursor will form a cavity structure inside the secondary particles aggregated by the primary particles during the synthesis process of the coprecipitation reaction, and the A element contained in the nickel source, cobalt source and M element carrier source will remain and adhere to the cavity structure as the cavity structure is formed. The A element remaining in the cavity can effectively regulate the cavity structure formed in the secondary particles to enrich the morphology of the cavity structure in the positive electrode material, and there is a positive correlation between the A element remaining in the cavity and the cavity rate in the secondary particles.

[0052] In some embodiments, the A element attached to the interior of the cavity structure includes at least sulfur, and the sulfur content in the positive electrode material is proportional to the cavity rate of the particle cross section. In step S1, the cavity rate in the nickel-cobalt precursor is modulated by adjusting the sulfur content of the nickel source, cobalt source and M element carrier in the coprecipitation reaction, so that the cavity rate and sulfur content of the secondary particle cross section of the obtained positive electrode material are in a suitable range, thereby enriching the cavity structure morphology inside the positive electrode material while improving the cycle life performance of the positive electrode material. For example, in one example, when the sulfur content in the positive electrode material is 0.01wt% to 0.35wt%, the positive electrode material has a cavity rate of 0.5% to 10%.

[0053] In some embodiments, the lithium source in step S2 can be selected from one or more of lithium carbonate, lithium phosphate, lithium dihydrogen phosphate, lithium acetate, lithium hydroxide, lithium oxide and lithium nitrate. Further, the lithium source can be selected from one or more of lithium carbonate, lithium hydroxide and lithium nitrate. Furthermore, the lithium source is lithium carbonate.

[0054] There is no particular limitation on the crushing method in step S2, and any crushing and grading method in the prior art may be used, such as a jet mill. The specific parameters for crushing the sintered product may be selected according to actual needs.

[0055] The present invention further provides a positive electrode plate, comprising a positive electrode current collector and a positive electrode active material layer disposed on the current collector, wherein the positive electrode active material layer comprises the positive electrode material of the present invention.

[0056] The preparation process of the positive electrode sheet is as follows: the positive electrode material, conductive agent and binder prepared above are mixed in a mass ratio of (90 to 99): 1.5: 1.5, preferably a mass ratio of 97: 1.5: 1.5, and a solvent N-methylpyrrolidone (NMP) is added, and the mixture is stirred and mixed to obtain a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector aluminum foil, and the positive electrode sheet is prepared through drying, cold pressing, slitting and other processes. Among them, the conductive agent can be selected from at least one of the conductive materials such as Super P (carbon black), acetylene black, carbon nanotubes (CNT), graphene, nano carbon fiber (VGCF), for example, the conductive agent is SP and CNT, and the mass ratio of SP and CNT is 1: 0.5; the binder can be selected from at least one of PVDF, PTFE, etc.

[0057] The present invention provides an electrochemical device, which includes the positive electrode material or positive electrode sheet of the present invention. The electrochemical device is, for example, a lithium-ion battery. Specifically, the lithium-ion battery includes a positive electrode sheet, a negative electrode sheet, a separator disposed between the positive electrode sheet and the negative electrode sheet, and an electrolyte.

[0058] Wherein, the positive electrode sheet is prepared by the preparation method described above in the present invention;

[0059] Preparation of negative electrode sheet: after mixing negative electrode materials such as graphite, conductive agent acetylene black, thickener CMC (sodium carboxymethyl cellulose) and binder SBR (styrene-butadiene rubber) in a mass ratio of 96.4:1:1.2:1.4, add deionized water, stir and mix thoroughly to obtain negative electrode slurry; evenly coat the negative electrode slurry on the negative electrode current collector copper foil, and prepare the negative electrode sheet through drying, cold pressing, slitting and other processes;

[0060] Diaphragm: The diaphragm is made of PE or PP porous membrane, preferably PP / PE / PP porous membrane, with a thickness of 9 μm to 18 μm, such as 9 μm, 12 μm, 16 μm or 18 μm; the air permeability is 180 s / 100 mL to 380 s / 100 mL, such as 180 s / 100 mL, 280 s / 100 mL or 380 s / 100 mL; the porosity is 30% to 50%, such as 30%, 40% or 50%.

[0061] Preparation of electrolyte: EC (ethylene carbonate), DMC (dimethyl carbonate) and EMC (ethyl methyl carbonate) are mixed in a mass ratio of 1:1:1 to obtain an organic solvent, and then the fully dried lithium salt LiPF6 is dissolved in the mixed organic solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0062] Assemble the battery: stack the prepared positive electrode sheet, separator, and negative electrode sheet in sequence, so that the separator is placed between the positive and negative electrode sheets to play a role of isolation. Then wrap it with aluminum plastic film, inject the above-prepared electrolyte after drying, and finally prepare a soft-pack battery (i.e., lithium-ion battery) with a capacity of 1Ah after packaging, standing, and formation.

[0063] The technical scheme of the present invention is described in detail below through several specific examples and comparative examples. Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available products or can be prepared by conventional methods in the art.

[0064] Example 1

[0065] Step 1, mixing nickel sulfate, cobalt sulfate and manganese sulfate solutions according to a Ni:Co:Mn molar ratio of 90:5:5, adding ammonia water and sodium hydroxide solution to the mixed salt solution for coprecipitation reaction, washing and drying the product after the coprecipitation reaction, wherein the prepared nickel-cobalt precursor is washed and dried and the sulfur content is 523 ppm;

[0066] Step 2, mixing the nickel-cobalt precursor with lithium hydroxide and 0.2 wt% ZrO2, and calcining in an oxygen atmosphere at a temperature of 760° C. for 12 hours to obtain a polycrystalline positive electrode material substrate;

[0067] Step 3: Mix the above-mentioned polycrystalline positive electrode material substrate with Al2O3 having a content ratio of 0.1wt%, and then sinter it in an oxygen atmosphere at a temperature of 400°C for 8h, and obtain a finished positive electrode material after crushing and grading.

[0068] Example 2

[0069] The difference between this embodiment and embodiment 1 is that in step 1, the sulfur concentration in the reactor during the coprecipitation reaction is adjusted so that the sulfur content of the nickel-cobalt precursor prepared in step 1 is 1345 ppm.

[0070] Example 3

[0071] The difference between this embodiment and embodiment 1 is that in step 1, the sulfur concentration in the reactor during the coprecipitation reaction is adjusted so that the sulfur content of the nickel-cobalt precursor prepared in step 1 is 2732 ppm.

[0072] Example 4

[0073] The difference between this embodiment and embodiment 1 is that in step 1, the sulfur concentration in the reactor during the coprecipitation reaction is adjusted so that the sulfur content of the nickel-cobalt precursor prepared in step 1 is 3209 ppm.

[0074] Example 5

[0075] The difference between this embodiment and embodiment 1 is that in step 1, the sulfur concentration in the reactor during the coprecipitation reaction is adjusted so that the sulfur content of the nickel-cobalt precursor prepared in step 1 is 5378 ppm.

[0076] Example 6

[0077] The difference between this embodiment and embodiment 1 is that in step 1, the sulfur concentration in the reactor during the coprecipitation reaction is adjusted so that the sulfur content of the nickel-cobalt precursor prepared in step 1 is 8427 ppm.

[0078] Example 7

[0079] The difference between this embodiment and embodiment 1 is that in step 1, the sulfur concentration in the reactor during the coprecipitation reaction is adjusted so that the sulfur content of the nickel-cobalt precursor prepared in step 1 is 2937 ppm.

[0080] Example 8

[0081] The difference between this embodiment and embodiment 1 is that: in step 1, the sulfur concentration in the reactor during the coprecipitation reaction is adjusted so that the sulfur content of the nickel-cobalt precursor prepared in step 1 is 2863ppm; in step 2, the nickel-cobalt precursor is mixed with lithium hydroxide, ZrO2 with a content ratio of 0.2wt% and Al2O3 with a content ratio of 0.2wt%, and calcined in an oxygen atmosphere at a temperature of 760°C for 12h; in step 3, the polycrystalline positive electrode material substrate obtained in step 2 is mixed with Al2O3 with a content ratio of 0.1wt% and TiO2 with a content ratio of 0.1wt%, and then sintered in an oxygen atmosphere at a temperature of 350°C for 8h, and the finished positive electrode material is obtained after crushing and grading.

[0082] Example 9

[0083] The difference between this embodiment and embodiment 1 is that: in step 1, the sulfur concentration in the reactor during the coprecipitation reaction is adjusted so that the sulfur content of the nickel-cobalt precursor prepared in step 1 is 2749ppm; in step 2, the nickel-cobalt precursor is mixed with lithium hydroxide, 0.2wt% ZrO2, 0.2wt% Al2O3, and 0.1wt% MgO, and calcined in an oxygen atmosphere at a temperature of 760°C for 12h; in step 3, the polycrystalline positive electrode material substrate obtained in step 2 is mixed with 0.1wt% Al2O3 and 0.1wt% B2O3, and then sintered in an oxygen atmosphere at a temperature of 350°C for 8h, and the finished positive electrode material is obtained after crushing and grading.

[0084] Example 10

[0085] The difference between this embodiment and embodiment 5 is that in step 1, the solutions of nickel sulfate, cobalt sulfate and manganese sulfate participating in the coprecipitation reaction are mixed according to the molar ratio of Ni:Co:Mn of 70:15:15.

[0086] Embodiment 11

[0087] The difference between this embodiment and embodiment 5 is that in step 1, the solutions of nickel sulfate, cobalt sulfate and manganese sulfate participating in the coprecipitation reaction are mixed according to the molar ratio of Ni:Co:Mn of 80:10:10.

[0088] Comparative Example 1

[0089] The difference between this embodiment and embodiment 8 is that in step 1, the sulfur concentration in the reactor during the coprecipitation reaction is adjusted so that the sulfur content of the nickel-cobalt precursor prepared in step 1 is 230 ppm.

[0090] Comparative Example 2

[0091] The difference between this embodiment and embodiment 9 is that in step 1, the sulfur concentration in the reactor during the coprecipitation reaction is adjusted so that the sulfur content of the nickel-cobalt precursor prepared in step 1 is 12027 ppm.

[0092] The nickel-cobalt precursors prepared in step S1 in Examples 1 to 11 and Comparative Examples 1 to 2 were tested for sulfur content. The precursor sulfur content testing method included: dissolving the nickel-cobalt precursor sample obtained in step S1 with hydrochloric acid, diluting it to a certain volume with water, and testing the sulfur content on an inductively coupled plasma mass spectrometer (ICP-MS).

[0093] The positive electrode sheets prepared in Examples 1 to 11 and Comparative Examples 1 to 2 were subjected to a sulfur content test on the cross section of the electrode particles and a cavity ratio test on the cross section of the electrode particles.

[0094] The test of the sulfur content in the cross section of the electrode particles comprises: using an ion beam to cut the electrode piece to obtain a cross-sectional sample of the electrode material, and using a high-resolution EDS test in a transmission electron microscope (TEM) to obtain the sulfur content of the cross-sectional sample.

[0095] The electrode particle cross-sectional cavity ratio test includes: the positive electrode cross-sectional SEM can be obtained by ion beam cutting the positive electrode sheet and then taking a SEM. In the SEM image, the cavity usually shows a different contrast from other physical areas. We can use graphics software to identify the cross-sectional area of ​​the cavity area and calculate the cavity ratio. This patent provides an example of a method for calculating the particle cross-sectional cavity ratio using the open source graphics software Image J:

[0096] Step a. First, obtain the cross section of the positive electrode sheet by ion beam cutting or other methods, select the particle cross section cut from the center of the secondary particle, and shoot a high-resolution SEM. The SEM shot must meet the requirements of uniform contrast distribution in other physical areas except for the cavity area;

[0097] Step b. Open the image using Image J and use the “split channels” function to separate the RGB channels to obtain a single-channel photo.

[0098] Step c. Setting the measurement scale according to the electron microscope scale; defining a circular (or elliptical or irregular) selected area, selecting the entire cross section of the secondary particle ball, and measuring the total area S1 of the selected area;

[0099] Step d. Adjust the image threshold until all the cavity areas of the particle cross section within the defined area are marked, and use the "analyze particle" function to obtain the total area S2 of the marked cavity areas;

[0100] Step e. Calculate the cavity ratio H = S2 / S1.

[0101] The positive electrode materials prepared in Examples 1 to 11 and the positive electrode materials prepared in Comparative Examples 1 to 2 were assembled into soft-pack batteries according to the assembly method of the present invention and subjected to battery performance tests, wherein the battery performance tests included cycle capacity retention tests and gas production performance tests.

[0102] The battery cycle capacity retention test includes: cycling at 25°C, 0.21A / g (calculated based on the mass of the positive electrode material), 2.8-4.25V charge and discharge mode. After 800 cycles, the discharge capacity of the battery at this time is divided by the discharge capacity of the first cycle, which is the battery's 800-cycle capacity retention rate.

[0103] The battery gas production performance test includes: testing the initial volume V0 of the battery cell after it is fully charged, then storing it in a 60°C high temperature cabinet, recharging and testing the volume every 7 days, and after 56 days, the cell volume is tested to be V2, and (V2-V1) / V1 is the gas production growth.

[0104] The test results of Examples 1 to 11 and Comparative Examples 1 to 2 are shown in Table 1.

[0105] Table 1: Structural properties and battery performance of positive electrode materials prepared in Examples 1 to 11 and Comparative Examples 1 to 2

[0106]

[0107]

[0108] By comparing Example 3, Example 8 and Comparative Example 1, it can be seen that when the sulfur content of the positive electrode cross section is too low (<0.01wt%), the positive electrode cross section cavity rate is low (<0.5%), the positive electrode material has a low capacity retention rate after 800 cycles, and the gas production increases greatly. This is because when the internal part of the positive electrode material is relatively dense as a whole, there is no cavity inside the secondary particles to buffer the stress generated by the volume expansion / contraction of the material during the charge and discharge process, resulting in the rupture of the secondary particles during the cycle, and the aggravation of the side reaction at the interface between the positive electrode and the electrolyte, resulting in poor cycle and gas production performance of the battery.

[0109] By comparing Example 4, Example 9 and Comparative Example 2, it can be found that when the sulfur content of the positive electrode cross section is too high (≥0.5wt%), there are too many cavities inside the secondary particles (positive electrode cross section cavity ratio ≥15%), and the tap density of the positive electrode material is also low. The particles are easily fractured during roller pressing, resulting in serious side reactions at the interface between the positive electrode and the electrolyte, causing the battery's cycle and gas production performance to deteriorate.

[0110] By comparing Example 5, Example 10 and Example 11, it can be found that when the sulfur content of the positive electrode cross section is the same, the adjustment of the component ratio between Ni, Co and Mn elements in the positive electrode material will not affect the tap density of the positive electrode material and the cycle and gas production performance of the secondary battery assembled with the positive electrode material.

[0111] In summary, the above cases show that when the sulfur content and the void ratio of the positive electrode cross section in the positive electrode material are distributed within a certain range, the material has good cyclability. This is because a certain proportion of the internal voids can buffer the volume strain of the positive electrode during the charge and discharge process and alleviate the rupture of secondary particles during the cycle. In contrast, when the sulfur content is too high or too low, and the internal void ratio of the positive electrode particles is too low or too high, it will affect the stress release of the material during the charge and discharge process, aggravate the side reactions at the interface between the electrode and the electrolyte, and lead to deterioration of the cycle and gas production performance.

[0112] The positive electrode material and its preparation method, positive electrode plate and electrochemical device in the present invention are based on the positive correlation between the A element content and the cavity rate in the positive electrode material particles. By introducing an appropriate proportion of the A element when the positive electrode material precursor is formed, the cavity structure formed inside the precursor is at an appropriate cavity rate, so as to ensure that the positive electrode material can buffer the volume strain during the charge and discharge process through the cavity structure with an appropriate proportion inside, and alleviate the rupture phenomenon of secondary particles during the cycle process, thereby improving the cycle life and volume energy density of the positive battery. Therefore, the present invention effectively overcomes some practical problems in the prior art and has high utilization value and use significance.

[0113] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A positive electrode material, characterized in that: The positive electrode material is a secondary particle formed by aggregation of primary particles, and the secondary particle contains a cavity structure.

2. The positive electrode material according to claim 1, characterized in that: The chemical formula of the positive electrode material is Li 1+a [Ni x Co y M z O 2-b A b , 0.7 ≤ x < 1, 0 ≤ y < 0.3, 0 ≤ z < 0.3, -0.2 < a < 0.2, 0 ≤ b < 0.2, x + y + z = 1; wherein, the M element includes one or more of Mn, Al, Ti, Zr, Mg, Sr, W, Mo, B, V, Se, Nb, Ru, Rh, Pd, Sb, Te, Ce, Ca, Zn, Y and W, and the A element includes one or more of F, N, Cl, S and P.

3. The positive electrode material according to claim 2, characterized in that: At least one element of the A elements is attached to the inner layer of the cavity structure.

4. The positive electrode material according to claim 3, characterized in that: The elements attached to the inner layer of the cavity structure include sulfur, and the cavity ratio of the positive electrode material is positively correlated with the content of the sulfur element in the positive electrode material.

5. The positive electrode material according to claim 2, characterized in that: When the sulfur content in the secondary particles is 0.01wt% to 0.35wt%, the positive electrode material has a cavity rate of 0.5% to 10%, and the particle tap density of the positive electrode material is 2.38 to 2.81g / cm 3 .

6. The positive electrode material according to claim 2 or 4, characterized in that: The valence state of the sulfur element in the positive electrode material is at least one of -2, +4 or +6; wherein the sulfur element is retained in the cavity structure in the form of at least one of sulfide ions, thiosulfate ions, sulfate ions and sulfite ions.

7. The positive electrode material according to claim 6, characterized in that: When the sulfur content in the secondary particles is 0.01wt% to 0.1wt%, the XPS photoelectron peak binding energy range of the sulfur in the positive electrode material is 168±2eV; When the sulfur content in the secondary particles is 0.01 wt % to 0.05 wt %, the XPS photoelectron peak binding energy range of the sulfur in the positive electrode material is 168.5±1 eV.

8. The positive electrode material according to claim 1, characterized in that: The inner diameter of the cavity structure is 10 nm to 1 μm.

9. A method for preparing a positive electrode material, characterized in that: include: A nickel source, a cobalt source and an M element carrier are mixed for a coprecipitation reaction to obtain a nickel-cobalt precursor material; wherein the M element includes one or more of Mn, Al, Ti, Zr, Mg, Sr, W, Mo, B, V, Se, Nb, Ru, Rh, Pd, Sb, Te, Ce, Ca, Zn, Y and W; and at least one element carrier among the nickel source, cobalt source and M source is sulfate. The nickel-cobalt precursor material is mixed with a lithium source and then sintered to obtain a positive electrode material; Wherein, the nickel-cobalt precursor forms a cavity structure inside the secondary particles during the coprecipitation reaction synthesis process.

10. The method for preparing the positive electrode material according to claim 9, characterized in that: The nickel source, cobalt source and M element carrier source include element A, and the element A includes one or more of F, N, Cl, S and P. During the coprecipitation reaction synthesis process of the nickel-cobalt precursor, the element A is attached to the inside of the cavity structure.

11. The method for preparing the positive electrode material according to claim 10, characterized in that: The sulfur element in the A element is attached to the inside of the cavity structure, and the cavity ratio of the positive electrode material is 0.5% to 10%.

12. An electrochemical device, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, characterized in that: The positive electrode plate comprises the positive electrode material described in any one of claims 1 to 8, or the positive electrode material prepared by the preparation method described in any one of claims 9 to 11.