Composite positive electrode and preparation method and application thereof

By using a modified composite ionic liquid on the positive electrode of the solid-state battery for vacuum impregnation, the interface contact between the positive electrode and the sulfide solid electrolyte is optimized, and the problem of poor contact between the traditional oxide positive electrode and the sulfide electrolyte is solved, which significantly improves the solid-state battery Capacity and rate performance.

CN118943367AInactive Publication Date: 2024-11-12GAO NENG SHI DAI (SHEN ZHEN) XIN NENG YUAN KE JI YOU XIAN GONG SI

Patent Information

Application Number
CN202410920758.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The poor contact between the traditional oxide positive electrode and the sulfide solid electrolyte leads to an increase in interface impedance, limiting the capacity and rate performance of solid-state batteries, especially under high-rate cycles.

Method used

Using composite positive electrodes, including positive electrode active materials, modified composite ionic liquids, solid electrolytes, conductive agents and binders, vacuum pressure-keeping impregnation is optimized for the positive electrode and sulfide solid electrolytes by dropping the modified composite ionic liquid on the positive electrode sheet. Interface contact reduces grain boundary impedance.

Benefits of technology

The capacity performance, rate performance and circulation performance of solid-state batteries have been significantly improved. Through the introduction of modified composite ion liquid, the conduction capacity and interface contact effect of lithium ions are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943367A_ABST
    Figure CN118943367A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of batteries, and discloses a composite positive electrode and a preparation method and application thereof. The composite positive electrode comprises the following components: a positive electrode active material, a modified composite ionic liquid, a solid electrolyte, a conductive agent and a binder, the modified composite ionic liquid comprises the following components: ionic liquid, hydrofluoroether and lithium salt. The non-polar hydrofluoroether diluent is introduced into the traditional ionic liquid, so that the viscosity of the ionic liquid is remarkably reduced, the capacity of the ionic liquid for rapidly conducting lithium ions is improved, the modified composite ionic liquid is obtained by matching with the lithium salt, the modified composite ionic liquid is introduced into the positive electrode of the sulfide solid-state battery, and the performance of the sulfide solid-state battery is improved. And the interface contact and grain boundary impedance of the positive electrode-sulfide solid electrolyte are optimized, so that the capacity exertion, rate capability and cycle performance of the solid-state battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries, and in particular relates to a composite positive electrode and a preparation method and application thereof. Background Art

[0002] At present, the commonly used solid electrolytes in solid-state lithium-ion batteries include polymer electrolytes, oxide electrolytes, sulfide solid electrolytes and halide electrolytes. Among them, sulfide solid electrolytes have the highest ionic conductivity (10 at room temperature). -3 ~10 -2 S / cm), and has the advantages of low hardness and good mechanical properties. It is considered to be the most promising type of solid electrolyte at present.

[0003] However, due to the large elastic modulus and poor deformation ability of traditional oxide positive electrodes, the contact between sulfide solid electrolytes and such electrode materials is poor, with an effective contact area of ​​less than 95%, which increases the interfacial impedance and thus degrades battery performance. In particular, under high-rate cycling, the battery capacity is severely limited. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a composite positive electrode and a preparation method and application thereof, which can optimize the interface contact with the sulfide solid electrolyte, reduce the grain boundary impedance, and thus improve the capacity, rate performance and cycle performance of the solid-state battery.

[0005] In a first aspect, the present invention provides a composite positive electrode, which comprises the following components: a positive electrode active material, a modified composite ionic liquid, a solid electrolyte, a conductive agent and a binder; the modified composite ionic liquid comprises the following components: an ionic liquid, a hydrofluoroether and a lithium salt.

[0006] In some embodiments of the present invention, the composite positive electrode includes the following components in mass percentage: 50% to 90% positive electrode active material, 0.5% to 30% modified composite ionic liquid, 5% to 35% solid electrolyte, 0.1% to 5% conductive agent and 0.1% to 5% binder.

[0007] In some embodiments of the present invention, the mass ratio of the ionic liquid to the hydrofluoroether is 1:(0.2-5), for example, it can be any point value among 1:0.2, 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, or a range value between any two point values; preferably, it is 1:(0.5-3).

[0008] In some embodiments of the present invention, the concentration of the lithium salt in the modified composite ionic liquid is 0.1 to 4 mol / L, for example, it can be any point value among 0.1 mol / L, 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, or a range value between any two point values; preferably, it is 0.5 to 2.5 mol / L.

[0009] In some embodiments of the present invention, the ionic liquid is composed of cations and anions, the cations include at least one of 1-ethyl-3-methylimidazolium ion, N-methyl, ethylpyrrolidium ion, N-methyl, propylpyrrolidium ion, N-methyl, butylpyrrolidium ion, N-methyl, ethylpiperidinium ion, N-methyl, propylpiperidinium ion and N-methyl, butylpiperidinium ion, and the anions include at least one of bisfluorosulfonyl imide ion and bistrifluoromethanesulfonyl imide ion.

[0010] In some embodiments of the present invention, the hydrofluoroether has the general structural formula R 1 -OR 2 , where the substituent R 1 and R 2 is an alkyl group or a fluorinated alkyl group having 1 to 9 carbon atoms, R 1 and R 2 The substituents may be the same or different, and at least one of the substituents is a fluorinated alkyl group.

[0011] In some embodiments of the present invention, the hydrofluoroether includes at least one of bis(2,2,2-trifluoroethyl) ether, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,1,2,3,3,3-pentafluoropropyl-2,2,2-trifluoroethyl ether, 1,1,2,3,3,3-hexafluoropropyl-2,2,2-trifluoroethyl ether and 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether.

[0012] In some embodiments of the present invention, the lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl imide), lithium bis(trifluoromethanesulfonyl imide), lithium difluorophosphate, lithium tetrafluoroborate, lithium trifluoromethanesulfonate, lithium bis(oxalatoborate), lithium difluorooxalatoborate and lithium difluorobis(oxalatophosphate).

[0013] In some embodiments of the present invention, the positive electrode active material includes at least one of lithium iron phosphate, lithium iron manganese phosphate, lithium cobaltate, lithium manganeseate, lithium nickelate, lithium nickel manganeseate, lithium nickel cobalt manganeseate, lithium nickel cobalt aluminum oxide and lithium-rich layered oxide.

[0014] In some embodiments of the present invention, the solid electrolyte is a sulfide solid electrolyte or a halide solid electrolyte; the sulfide solid electrolyte includes thio-LISICON, Li 10 G 2 S 12 , Li 10 SiP 2 S 12 , Li 3 PS 4 , Li 7 P 3 S 11 and Li 7-a PS 6-a X a At least one of the following, wherein X is at least one of Cl, Br and I, and a is 0.5 to 2; the halide solid electrolyte is Li a MX b , wherein M is selected from at least one of Al, Y, Ga, In, Er, Sc, Ti, Zr and La, X is selected from at least one of F, Cl, Br and I, 0≤a≤10, 1≤b≤13;

[0015] In some embodiments of the present invention, the conductive agent includes at least one of graphite, acetylene black, graphene, graphyne, carbon nanotubes, carbon fibers and carbon black.

[0016] In some embodiments of the present invention, the binder includes at least one of polyvinylidene fluoride, polyvinylidene fluoride copolymer, polytetrafluoroethylene, polyacrylate, polyethylene acetate, hydrogenated styrene-butadiene copolymer, ethylene acrylate copolymer, styrene-butadiene rubber, nitrile rubber and hydrogenated nitrile rubber.

[0017] In a second aspect of the present invention, a method for preparing the composite positive electrode according to the first aspect of the present invention is provided, comprising the following steps:

[0018] The positive electrode active material, solid electrolyte, conductive agent and binder are mixed, ground and dry pressed to obtain a positive electrode sheet;

[0019] The ionic liquid, hydrofluoroether and lithium salt are mixed to prepare a modified composite ionic liquid;

[0020] The modified composite ionic liquid is dripped onto the positive electrode sheet, and vacuum pressure is maintained for impregnation to obtain the composite positive electrode.

[0021] In some embodiments of the present invention, the amount of the modified composite ionic liquid added is 5% to 25% of the mass of the positive electrode sheet, for example, it can be any point value among 5%, 10%, 15%, 20%, 25%, or a range value between any two point values; preferably, it is 10% to 20%.

[0022] In some embodiments of the present invention, the specific process for preparing the modified composite ionic liquid is: dissolving a lithium salt in an ionic liquid solvent to obtain a composite ionic liquid, then adding a hydrofluoroether diluent, and mixing uniformly to obtain a modified composite ionic liquid.

[0023] In some embodiments of the present invention, the thickness of the positive electrode sheet is 120-140 μm.

[0024] In some embodiments of the present invention, the vacuum pressure impregnation time is 1 to 3 hours. The present invention adopts vacuum pressure impregnation and preferably selects a suitable time, so that after vacuum pressure impregnation, the modified composite ionic liquid can fully enter the internal pores of the positive electrode sheet, and there is no residue on the surface, which further improves the performance of the composite positive electrode.

[0025] According to a third aspect of the present invention, a solid-state battery is provided, wherein the solid-state battery comprises the composite positive electrode according to the first aspect of the present invention.

[0026] In some embodiments of the present invention, the solid-state battery further comprises a solid electrolyte layer and a negative electrode.

[0027] In some embodiments of the present invention, the solid electrolyte layer uses a sulfide solid electrolyte, and the sulfide solid electrolyte includes thio-LISICON, Li 10 G 2 S 12 , Li 10 SiP 2 S 12 , Li 3 PS 4 , Li 7 P 3 S 11 and Li 7-a PS 6-a X a At least one of the following, wherein X is at least one of Cl, Br and I, and a is 0.5-2.

[0028] In some embodiments of the present invention, the negative electrode includes at least one of graphite, silicon-based materials, silver-carbon composite materials, lithium titanate, metallic lithium, metallic indium, and lithium alloys.

[0029] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0030] The present invention introduces a non-polar hydrofluoroether diluent into a traditional ionic liquid, thereby significantly reducing the viscosity of the ionic liquid, improving its ability to quickly conduct lithium ions, and adding a lithium salt to obtain a modified composite ionic liquid. By introducing the modified composite ionic liquid into the positive electrode of a sulfide solid-state battery, the interface contact and grain boundary impedance of the positive electrode-sulfide solid electrolyte are optimized, thereby improving the capacity, rate performance and cycle performance of the solid-state battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The first cycle 0.1C charge and discharge curves of the solid-state batteries of Example 1, Comparative Example 1, and Comparative Example 2 are shown. DETAILED DESCRIPTION

[0032] The present invention is further described in detail below by specific examples. The raw materials, reagents or devices used in the examples can be obtained from conventional commercial sources or by prior art methods unless otherwise specified. Unless otherwise specified, the experiments or test methods are conventional methods in the art.

[0033] Example 1: Preparation of composite positive electrode and solid-state battery

[0034] The composite positive electrode in this example is prepared by the following preparation method, and the specific steps are as follows:

[0035] (1) Preparation of modified composite ionic liquids

[0036] Dissolving lithium bis(fluorosulfonyl)imide in N-methyl-propylpyrrolidine bis(fluorosulfonyl)imide ionic liquid solvent to obtain a composite ionic liquid, and then adding 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether diluent, mixing evenly to obtain a modified composite ionic liquid; wherein the mass ratio of the ionic liquid solvent to the diluent is 1:1, and the concentration of lithium bis(fluorosulfonyl)imide in the modified composite ionic liquid is 1 mol / L;

[0037] (2) Preparation of composite positive electrode

[0038] LiNi 0.8 Co 0.1 Mn 0.1 O 2 Positive electrode active material, Li 6 PS 5 The Cl solid electrolyte, carbon nanofibers, and polytetrafluoroethylene were weighed in a mortar at a mass ratio of 75:22:2:1, ground for 15 minutes, and then pressed into a positive electrode sheet with a thickness of 130 μm using a dry method. The modified composite ionic liquid obtained in step (1) was then dripped onto the positive electrode sheet in an amount of 20% of the mass of the positive electrode sheet. After vacuum pressure impregnation for 2 hours, a composite positive electrode was obtained.

[0039] The solid-state battery in this example is prepared by the following preparation method, and the specific steps are as follows:

[0040] The composite positive electrode, Li 6 PS 5 The Cl solid electrolyte powder and the Li-In metal foil negative electrode were placed into a solid-state battery mold in sequence and pressed at a pressure of 450 MPa to produce a solid-state battery.

[0041] Example 2: Preparation of composite positive electrode and solid-state battery

[0042] The composite positive electrode in this example is prepared by the following preparation method, and the specific steps are as follows:

[0043] (1) Preparation of modified composite ionic liquids

[0044] Dissolving lithium bis(fluorosulfonyl)imide in N-methyl-propylpyrrolidine bis(fluorosulfonyl)imide ionic liquid solvent to obtain a composite ionic liquid, and then adding 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether diluent, mixing evenly to obtain a modified composite ionic liquid; wherein the mass ratio of the ionic liquid solvent to the diluent is 1:2, and the concentration of lithium bis(fluorosulfonyl)imide in the modified composite ionic liquid is 1 mol / L;

[0045] (2) Preparation of composite positive electrode

[0046] LiNi 0.8 Co 0.1 Mn 0.1 O 2 Positive electrode active material, Li 6 PS 5 The Cl solid electrolyte, carbon nanofibers, and polytetrafluoroethylene were weighed in a mortar at a mass ratio of 75:22:2:1, ground for 15 minutes, and then pressed into a positive electrode sheet with a thickness of 130 μm using a dry method. The modified composite ionic liquid obtained in step (1) was then dripped onto the positive electrode sheet in an amount of 20% of the mass of the positive electrode sheet. After vacuum pressure impregnation for 2 hours, a composite positive electrode was obtained.

[0047] The solid-state battery in this example is prepared by the following preparation method, and the specific steps are as follows:

[0048] The composite positive electrode, Li 6 PS 5 The Cl solid electrolyte powder and the Li-In metal foil negative electrode were placed into a solid-state battery mold in sequence and pressed at a pressure of 450 MPa to produce a solid-state battery.

[0049] Example 3: Preparation of composite positive electrode and solid-state battery

[0050] The composite positive electrode in this example is prepared by the following preparation method, and the specific steps are as follows:

[0051] (1) Preparation of modified composite ionic liquids

[0052] Dissolving lithium bis(fluorosulfonyl)imide in N-methyl-propylpyrrolidine bis(fluorosulfonyl)imide ionic liquid solvent to obtain a composite ionic liquid, and then adding 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether diluent, mixing evenly to obtain a modified composite ionic liquid; wherein the mass ratio of the ionic liquid solvent to the diluent is 1:1, and the concentration of lithium bis(fluorosulfonyl)imide in the modified composite ionic liquid is 2 mol / L;

[0053] (2) Preparation of composite positive electrode

[0054] LiNi 0.8 Co 0.1 Mn 0.1 O 2 Positive electrode active material, Li 6 PS 5 The Cl solid electrolyte, carbon nanofibers, and polytetrafluoroethylene were weighed in a mortar at a mass ratio of 75:22:2:1, ground for 15 minutes, and then pressed into a positive electrode sheet with a thickness of 130 μm using a dry method. The modified composite ionic liquid obtained in step (1) was then dripped onto the positive electrode sheet in an amount of 20% of the mass of the positive electrode sheet. After vacuum pressure impregnation for 2 hours, a composite positive electrode was obtained.

[0055] The solid-state battery in this example is prepared by the following preparation method, and the specific steps are as follows:

[0056] The composite positive electrode, Li 6 PS 5 The Cl solid electrolyte powder and the Li-In metal foil negative electrode were placed into a solid-state battery mold in sequence and pressed at a pressure of 450 MPa to produce a solid-state battery.

[0057] Comparative Example 1 (the only difference from Example 1 is that no modified composite ionic liquid is added)

[0058] The positive electrode in this example is prepared by the following preparation method, the specific steps are:

[0059] LiNi 0.8 Co 0.1 Mn 0.1 O 2 Positive electrode active material, Li 6 PS 5 Cl solid electrolyte, carbon nanofibers, and polytetrafluoroethylene were weighed in a mortar at a mass ratio of 80:17:2:1, ground for 15 min, and then dry-pressed into a positive electrode with a thickness of 130 μm.

[0060] The solid-state battery in this example is prepared by the following preparation method, and the specific steps are as follows:

[0061] The positive electrode and Li 6 PS 5 The Cl solid electrolyte powder and the Li-In metal foil negative electrode were placed into a solid-state battery mold in sequence and pressed at a pressure of 450 MPa to produce a solid-state battery.

[0062] Comparative Example 2 (the only difference from Example 1 is that no hydrofluoroether diluent modification is added)

[0063] The composite positive electrode in this example is prepared by the following preparation method, and the specific steps are as follows:

[0064] (1) Preparation of composite ionic liquids

[0065] Dissolving lithium bis(fluorosulfonyl)imide in N-methyl-propylpyrrolidine bis(fluorosulfonyl)imide ionic liquid solvent to obtain a composite ionic liquid; wherein the concentration of lithium bis(fluorosulfonyl)imide in the composite ionic liquid is 1 mol / L;

[0066] (2) Preparation of composite positive electrode

[0067] LiNi 0.8 Co 0.1 Mn 0.1 O 2 Positive electrode active material, Li 6 PS 5 The Cl solid electrolyte, carbon nanofibers, and polytetrafluoroethylene were weighed in a mortar at a mass ratio of 75:22:2:1, ground for 15 minutes, and then pressed into a positive electrode sheet with a thickness of 130 μm using a dry method. The composite ionic liquid obtained in step (1) was then dripped onto the positive electrode sheet in an amount of 20% of the mass of the positive electrode sheet. After vacuum pressure impregnation for 2 hours, a composite positive electrode was obtained.

[0068] The solid-state battery in this example is prepared by the following preparation method, and the specific steps are as follows:

[0069] The composite positive electrode, Li 6 PS 5 The Cl solid electrolyte powder and the Li-In metal foil negative electrode were placed into a solid-state battery mold in sequence and pressed at a pressure of 450 MPa to produce a solid-state battery.

[0070] Product effect testing

[0071] The solid-state batteries prepared in the embodiments and comparative examples were used as test samples. The test method was as follows: the solid-state batteries were placed in a 25°C constant temperature box for testing. The first cycle charge and discharge rate was 0.1C, and then the cycle test was performed at a rate of 0.3C. The voltage range was 2.2 to 3.7V (2.8 to 4.3V vs. Li+ / Li). The test results are shown in Table 1. The first cycle 0.1C charge and discharge curves of the solid-state batteries of Embodiment 1, Comparative Example 1, and Comparative Example 2 are shown in Table 1. Figure 1 shown.

[0072] Table 1

[0073]

[0074] It can be seen from the above test results that compared with the solid-state battery of the comparative example, the capacity performance, rate performance and cycle performance of the solid-state battery prepared in the embodiment of the present invention are significantly better.

[0075] The preferred embodiments of the present invention are specifically described above, but the invention is not limited to the embodiments. Those skilled in the art may make various equivalent modifications or substitutions without violating the spirit of the invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.

Claims

1. A composite positive electrode, It is characterized in that The composite positive electrode comprises the following components: positive electrode active material, modified composite ionic liquid, solid electrolyte, conductive agent and binder; the modified composite ionic liquid comprises the following components: ionic liquid, hydrofluoroether and lithium salt.

2. The composite positive electrode according to claim 1, It is characterized in that The composite positive electrode comprises the following components in percentage by mass: 50% to 90% of positive electrode active material, 0.5% to 30% of modified composite ionic liquid, 5% to 35% of solid electrolyte, 0.1% to 5% of conductive agent and 0.1% to 5% of binder.

3. The composite positive electrode according to claim 1, It is characterized in that The mass ratio of the ionic liquid to the hydrofluoroether is 1:(0.2-5).

4. The composite positive electrode according to claim 1, It is characterized in that The concentration of the lithium salt in the modified composite ionic liquid is 0.1-4 mol / L.

5. The composite positive electrode according to claim 1, It is characterized in that The ionic liquid is composed of cations and anions, wherein the cations include at least one of 1-ethyl-3-methylimidazolium ion, N-methyl, ethylpyrrolidium ion, N-methyl, propylpyrrolidium ion, N-methyl, butylpyrrolidium ion, N-methyl, ethylpiperidinium ion, N-methyl, propylpiperidinium ion and N-methyl, butylpiperidinium ion, and the anions include at least one of bisfluorosulfonyl imide ion and bistrifluoromethanesulfonyl imide ion.

6. The composite positive electrode according to claim 1, It is characterized in that The general structural formula of the hydrofluoroether is R 1 -OR 2 , where the substituent R 1 and R 2 is an alkyl group or a fluorinated alkyl group having 1 to 9 carbon atoms, R 1 and R 2 The substituents may be the same or different, and at least one of the substituents is a fluorinated alkyl group.

7. The composite positive electrode according to claim 1, It is characterized in that The lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl imide), lithium bis(trifluoromethanesulfonyl imide), lithium difluorophosphate, lithium tetrafluoroborate, lithium trifluoromethanesulfonate, lithium bis(oxalatoborate), lithium difluorooxalatoborate and lithium difluorobis(oxalatophosphate).

8. A method for preparing a composite positive electrode according to any one of claims 1 to 7, It is characterized in that The following steps are involved: The positive electrode active material, solid electrolyte, conductive agent and binder are mixed, ground and dry pressed to obtain a positive electrode sheet; The ionic liquid, hydrofluoroether and lithium salt are mixed to prepare a modified composite ionic liquid; The modified composite ionic liquid is dripped onto the positive electrode sheet, and vacuum pressure is maintained for impregnation to obtain the composite positive electrode.

9. The preparation method according to claim 8, It is characterized in that The vacuum pressure-maintaining impregnation time is 1 to 3 hours.

10. A solid-state battery, It is characterized in that The solid-state battery comprises the composite positive electrode according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Solid-state battery positive electrode material, production method for solid-state battery positive electrode material, all-solid-state lithium-sulfur battery using solid-state battery positive electrode material, and production method for all-solid-state lithium-sulfur battery using solid-state battery positive electrode material

    CN108780880A

  • Improved composite positive electrode for solid-state lithium-sulfur battery and preparation method thereof

    CN111952551A

  • Thin solid electrolyte with high ionic conductivity

    CN116565303A

  • Positive electrode active material layer for solid-state battery

    JP2020038771A

  • KR20240036042A

Cited By

  • Solid-state battery cell, positive electrode sheet, battery device, energy storage device, and electric device

    WO2026137657A1