Fuel cell PtPdRuCuBi high-entropy alloy electrocatalyst and application thereof

By using polyol-high-temperature injection method to prepare PtPdRuCuBi high-entropy alloy nanoelectrocatalysts in direct ethanol fuel cells, the problem of insufficient catalyst activity and stability is solved, and efficient ethanol catalytic performance and the sustainability of fuel cells are improved.

CN118943398APending Publication Date: 2024-11-12CHINA THREE GORGES UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411093572.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing direct ethanol fuel cell catalysts have insufficient activity and stability in the catalytic ethanol oxidation process, which affects the efficiency and sustainability of the fuel cell.

Method used

PtPdRuCuBi high-entropy alloy nanoelectrocatalyst was prepared by polyol-high-temperature injection method. P123 and triethylene glycol were used as reducing agents and protective agents to form a five-membered alloy electrocatalyst with a chain structure, improving the stability and activity of the catalyst.

Benefits of technology

The catalytic activity and stability of the catalyst are significantly improved, excellent ethanol catalytic performance is achieved, and the conversion efficiency and sustainability of fuel cells are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943398A_ABST
    Figure CN118943398A_ABST
Patent Text Reader

Abstract

The invention provides a Bi-based fuel cell PtPdRuCuBi high-entropy alloy electrocatalyst. The alloy electrocatalyst has a characteristic chain structure, the nano chain size is uniform, the average particle size of the catalyst is about 10.35 + / -0.17 nm, and the specific active current density is 800.3 mA. Mg <-1 > Pt. The preparation method comprises the following steps: weighing P123, dissolving the P123 in TEG, ultrasonically dispersing to be uniform, heating to 230 DEG C in a stirring reflux state, dropwise adding a precursor TEG solution of five elements at a constant speed within 30 minutes, and stopping heating after dropwise adding until the solution completely becomes black; and cooling to room temperature, and sequentially carrying out centrifugal washing with water, absolute ethyl alcohol and acetone to obtain the fuel cell PtPdRuCuBi alloy electrocatalyst. The prepared catalyst has excellent performance of electrocatalytic oxidation of ethanol, and has great application and development prospects in direct ethylene glycol fuel cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fuel cells and relates to a method for preparing an anode catalyst, in particular to a method for preparing a PtPdRuCuBi high entropy alloy electrocatalyst for a direct ethanol fuel cell. Background Art

[0002] Proton exchange membrane fuel cell (PEMFC) is a highly efficient conversion device that converts chemical energy stored in fuel into electrical energy. It does not go through a thermal engine process and is not limited by the Carnot cycle. It has a very high conversion efficiency and is rated as one of the most promising emerging energy conversion devices. As long as the raw materials are replenished, electrical energy can be continuously output to the external circuit. Direct ethanol fuel cell (DEFC) is a type of proton exchange membrane fuel cell. It has the advantages of simple structure, high theoretical specific density, low toxicity of fuel, safe and easy storage and transportation, and can be obtained in large quantities only by organic fermentation containing sugars. It is a non-toxic, environmentally friendly and renewable fuel. Once successfully developed, it has a very broad prospect. . Summary of the invention

[0003] In the present invention, by preparing a chain-structured PtPdRuCuBi high-entropy alloy nano-electrocatalyst, the high entropy property can increase the disorder of the system, thereby showing a lower Gibbs free energy, significantly improving the stability of the catalyst. The synergistic effect of the components affects the overall performance, thereby improving the catalytic activity of the catalyst.

[0004] In the present invention, a polyol-high temperature injection method is adopted, triethylene glycol is used as a reducing agent, P123 is used as a reducing agent and a protecting agent, and a five-element PtPdRuCuBi alloy electrocatalyst with uniform nanochain distribution is prepared under the condition of a 230° C. oil bath.

[0005] The purpose of the present invention is to improve the catalytic activity and stability of the catalyst through the high entropy effect of the catalyst and the synergistic effect of each component, and to prepare a fuel cell PtPdRuCuBi nano-electrocatalyst with excellent ethanol catalytic performance.

[0006] The atomic proportion of each element in the alloy electrocatalyst is between 5 and 35%, the elements are evenly distributed, and the alloy catalyst has a chain structure.

[0007] In some preferred cases, the atomic proportion of each element in Pt, Pd, Ru, and Cu in the alloy electrocatalyst is between 5% and 35%, and the atomic proportion of Bi is 15-20%.

[0008] Furthermore, the atomic ratios of Pt, Pd, Ru, Cu and Bi in the alloy electrocatalyst are approximately 16.83%, 28.78%, 23.34%, 10.54% and 19.51%, respectively. The alloy electrocatalyst has a nanochain structure and an average particle size of about 10.35±0.17nm.

[0009] The technical solution adopted by the present invention to achieve the above-mentioned purpose is as follows: (1) Weigh P123 (PEO 19 -PPO 69 -PEO 19 ) was dissolved in triethylene glycol (TEG) and ultrasonically dispersed until uniform. The solution was transferred to a three-necked flask. Under nitrogen saturation conditions, magnetic stirring was accompanied by a temperature increase process. The condensed water was heated in an oil bath to reflux to 200-230°C. A TEG mixed solution of K2PtCl6, K2PdCl4, CuCl2·2H2O,RuCl2·H2O-x, BiN3O9·5H2O) that had been ultrasonically dispersed uniformly was dripped into it. The flow rate was controlled to drip slowly drop by drop (so that the elements were reduced at the same time). The mixed solution gradually turned black. After the addition was completed, the heating was stopped. The solution had completely turned black with the formation of precipitation.

[0010] The mixture was naturally cooled to room temperature, and then centrifuged and washed 3 to 4 times with deionized water, anhydrous ethanol, and acetone at 8000 to 10000 rpm / min, respectively, to obtain a PtPdRuCuBi alloy electrocatalyst for a fuel cell.

[0011] In step (1), P123 is dissolved in TEG; in step (2), the two precursor salts are dissolved in TEG respectively.

[0012] In the steps of the present invention, TEG is a reducing agent; P123 is a reducing agent and a protecting agent. During the centrifugal washing process, the catalyst is first washed with double distilled water for 3 to 4 times, and then washed with anhydrous ethanol and acetone for 3 to 4 times to ensure that the unreacted reactants are removed from the catalyst surface.

[0013] The mass ratio of P123, K2PtCl6, K2PdCl4, CuCl2, RuCl2·H2O-x, and BiN3O9·5H2O is approximately 1: 0.005-0.035: 0.005-0.035: 0.005-0.035: 0.005-0.035: 0.005-0.035.

[0014] In some preferred embodiments, the mass ratio of P123, K2PtCl6, K2PdCl4, CuCl2, RuCl2·H2O-x, and BiN3O9·5H2O is approximately 1: 0.005-0.035: 0.005-0.035: 0.005-0.035: 0.005-0.035: 0.01-0.030.

[0015] The fuel cell PtPdRuCuBi alloy electrocatalyst has a characteristic chain structure, the nanochain size is uniform, the average catalyst particle size is about 10.35±0.17nm, and the specific active current density is 800.3 mA·mg -1 P t above.

[0016] The fuel cell PtPdRuCuBi alloy electrocatalyst has a chain structure and high entropy characteristics, which effectively improves the catalytic performance and stability of the PtPdRuCuBi nano electrocatalyst.

[0017] The PtPdRuCuBi alloy electrocatalyst for fuel cells and the preparation method thereof involved in the present invention have the following significant features: (1) The preparation method is simple and does not require any special equipment. It can be achieved by using wet chemical methods under relatively simple conditions to simultaneously reduce five elements (including precious metals and non-precious metal elements with large differences in reduction potential) to form an alloy.

[0018] (2) P123 acts as both a reducing agent and a protective agent, and TEG acts as a reducing agent and a solvent. The experiment is low-cost, green and safe.

[0019] (3) The prepared catalyst has excellent electrocatalytic ethanol oxidation performance and stability, and has great application and development prospects in direct ethanol fuel cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a transmission electron microscope image of the fuel cell PtPdRuCuBi electrocatalyst prepared in Example 1, wherein Figure 1 a, b are TEM images of the catalyst, and the inset in b is the particle size distribution of the catalyst; Figure 1 c and d are HRTEM images.

[0021] Figure 2 Element distribution diagram of the fuel cell PtPdRuCuBi electrocatalyst prepared in Example 1, Figure 2 a is a high-angle annular dark field scanning transmission image (HAADF-STEM), Figure 2 b is the mapping diagram, and c~h correspond to the distribution diagram and overlapping diagram of the five elements respectively.

[0022] Figure 3 Cyclic voltammetry curves of the fuel cell electrocatalyst prepared in Examples 1 and 2 and commercial Pt / C for electrocatalytic oxidation of ethanol.

[0023] Figure 4 The chronoamperometric curves of the fuel cell electrocatalysts prepared in Examples 1 and 2 and the commercial Pt / C electrocatalytic oxidation of ethanol are shown.

[0024] Figure 5 This is a CV curve diagram of 500 cycles of electrocatalytic oxidation of ethanol by the fuel cell prepared in Examples 1 and 2. DETAILED DESCRIPTION

[0025] The present invention will be further described below in conjunction with the accompanying drawings and specific implementation cases. It should be stated here that these implementation cases are only used to illustrate the present invention rather than to limit the scope of the present invention. After reading the present invention, modifications to various equivalent forms by those skilled in the art all fall within the scope defined by the claims attached to this application.

[0026] Example 1 (1) Dissolve 0.09 mmol P123 (about 522 mg) in 30 mL triethylene glycol (TEG) and stir ultrasonically for 20 min until it is completely dissolved. This is referred to as solution A. Transfer solution A to a three-necked flask. After sealing the system, exhaust the air and inject N2. Repeat this process three times. Transfer the system to an oil bath and heat the solution to 230°C.

[0027] (2) A mixture of five metal precursors (K2PtCl6, K2PdCl4, CuCl2·2H2O, RuCl2-H2O-x, BiN3O9·5H2O) in equimolar amounts (0.03 mmol) was completely dissolved in TEG (10 mL) to prepare solution B. Solution B was injected into solution A and the injection was completed within 30 min. The temperature of solution A was maintained at 230 ± 5°C while injecting solution B. After the injection of solution B was completed, the heating was stopped.

[0028] (3) Cool naturally to room temperature and keep it still. Centrifuge the black turbid liquid obtained after the reaction at 10000 r / min, wash it with deionized water for 4 times, and then wash it with a mixed solution of anhydrous ethanol and acetone for 4 times (to remove excess P123 and TEG). Finally, add anhydrous ethanol to disperse and protect the product to obtain the fuel cell PtPdRuCuBi alloy electrocatalyst.

[0029] (4) The PtPdRuCuBi alloy electrocatalyst prepared in this example was modified on a glassy carbon electrode to prepare a working electrode, and cyclic voltammetry and chronoamperometry tests were performed on it. The test conditions were: the solution was a nitrogen-saturated 1 mol / L KOH+1 mol / L EtOH solution, the CV scan range was -0.9-0.3 V (vs. SCE), the scan rate was 50 mV / s, and the potential value was converted to the standard hydrogen electrode potential, which can be converted by the following formula: E(RHE) = E(SCE)+0.0591*pH+0.242. The scan rate was 50 mV / s, the it potential was -0.2 V (vs SCE), and the test results are shown in Figure 3 and Figure 4 middle.

[0030] Figure 1 and Figure 2 The transmission electron microscope (TEM) image and element distribution map of the fuel cell PtPdRuCuBi alloy electrocatalyst prepared in Example 1. As can be seen from Figure 1, the prepared catalyst structure is distributed in a chain-like manner, the nanochain is relatively short, and there is a slight agglomeration phenomenon. The average particle size is about 10.35±0.17nm, and the element distribution is Figure 5 The elements are evenly distributed, indicating good alloying. The contents of Pt, Pd, Ru, Cu, and Bi in the final catalyst are 16.83%, 28.78%, 23.34%, 10.54%, and 19.51%, respectively.

[0031] Depend on Figure 3 It can be seen that the PtPdRuCuBi alloy electrocatalyst prepared in Example 1 exhibits good ethanol oxidation activity. The electrocatalytic methanol oxidation activity of Example 1 is significantly better than that of Example 2 and the commercial Pt / C nanocatalyst, with a mass current density of about 800.3 mA·mg -1 Pt , which is 2.74 times that of commercial Pd black.

[0032] Example 2 (1) Dissolve 0.09 mmol P123 (about 522 mg) in 30 mL triethylene glycol (TEG) and stir ultrasonically for 20 min until it is completely dissolved. This is referred to as solution A. Transfer solution A to a three-necked flask. After sealing the system, exhaust the air and inject N2. Repeat this process three times. Transfer the system to an oil bath and heat the solution to 230°C.

[0033] (2) A mixture of equimolar amounts (0.03 mmol) of four metal precursors (K2PtCl6, K2PdCl4, CuCl2·2H2O, RuCl2-H2O-x) was completely dissolved in TEG (10 mL) to prepare solution B. Solution B was injected into solution A and the injection was completed within 30 min. The temperature of solution A was maintained at 230 ± 5°C while injecting solution B. After the injection of solution B was completed, the heating was stopped.

[0034] (3) Cool naturally to room temperature and keep it still. Centrifuge the black turbid liquid obtained after the reaction at 10000 r / min, wash it with deionized water for 4 times, and then wash it with a mixed solution of anhydrous ethanol and acetone for 4 times (to remove excess P123 and TEG). Finally, add anhydrous ethanol to disperse and protect the product to obtain the PtPdRuCu alloy electrocatalyst for fuel cells.

[0035] (4) The PtPdRuCu alloy electrocatalyst prepared in this example was modified on a glassy carbon electrode to prepare a working electrode, and cyclic voltammetry and chronoamperometry tests were performed on it. The test conditions were: the solution was a nitrogen-saturated 1 mol / L KOH+1 mol / L EtOH solution, the CV scan range was -0.9-0.3 V (vs. SCE), the scan rate was 50 mV / s, and the potential value was converted to the standard hydrogen electrode potential, which can be converted by the following formula: E(RHE) = E(SCE)+0.0591*pH+0.242. The scan rate was 50 mV / s, the it potential was -0.2 V (vs SCE), and the test results are shown in Figure 3 and Figure 4 middle.

[0036] Depend on Figure 4 The chronoamperometric curves of Example 1, Example 2 and commercial Pt / C show that the stability of the PtPdRuCu and PtPdRuCuBi alloy electrocatalysts prepared in Example 1 is significantly better than that of commercial Pt / C.

[0037] Figure 5 The accelerated aging tests also showed the ultrahigh stability of PtPdRuCu and PtPdRuCuBi alloys. Figure 5 As shown in b, the positive sweep peak current density jb of the PtPdRuCuBi catalyst prepared in Example 1 after 500 CV cycles only increased from 794.5 mA·mg -1 Pt Down to 784.1 mA·mg -1 Pt , the catalytic activity was retained by 98.7%, with almost no loss. Figure 5As shown in a, the activity of the PtPdRuCu catalyst prepared in Example 2 gradually increased within 200 cycles and then decreased slightly. Specifically, the current density of the first cycle was 687.8 mA·mg -1 Pt , increased to 792.1 mA·mg at the 200th cycle -1 Pt , and then decreased to 715.5 mA·mg at the 500th lap -1 Pt .

[0038] When the Bi content increases to 2 times, Bi oxides appear, and the activity of the catalyst decreases, and the mass current density decreases to 650.35 mA·mg -1 Pt When the Bi content is reduced to 0.5 times, the catalytic function of Bi is weakened, and the activity of the catalyst is also reduced, and the mass current density is reduced to 680.46 mA·mg -1 Pt .

Claims

1. A PtPdRuCuBi high entropy alloy electrocatalyst for a fuel cell, characterized in that: The atomic proportion of each element in the alloy electrocatalyst is between 5 and 35%, the elements are evenly distributed, and the alloy catalyst has a chain structure.

2. The fuel cell PtPdRuCuBi alloy electrocatalyst according to claim 1, characterized in that: The atomic proportion of each element in Pt, Pd, Ru, and Cu in the alloy electrocatalyst is between 5 and 35%, and the proportion of Bi is 15-20%.

3. The method for preparing a PtPdRuCuBi high entropy alloy electrocatalyst for a fuel cell according to claim 1 or 2, characterized in that: The preparation method is as follows: (1) Weigh P123 and dissolve it in triethylene glycol, disperse it uniformly by ultrasonication, and uniformly add the TEG mixed solution of the metal precursor dropwise under stirring, heating and reflux. After the addition is complete, stop heating and the solution has completely turned black. The metal precursor is a mixed solution containing K2PtCl6, K2PdCl4, CuCl2·2H2O, RuCl2·H2O-x, and BiN3O9·5H2O; (2) After the reaction is completed, the mixture is cooled to room temperature and washed by centrifugation with water, anhydrous ethanol and acetone in sequence to obtain a PtPdRuCuBi high entropy alloy electrocatalyst for a fuel cell.

4. The method for preparing the PtPdRuCuBi high entropy alloy electrocatalyst for fuel cells according to claim 3, characterized in that: The mass ratio of P123, K2PtCl6, K2PdCl4, CuCl2, RuCl2·H2O-x, and BiN3O9·5H2O is approximately 1: 0.005-0.035: 0.005-0.035: 0.005-0.035: 0.005-0.035: 0.005-0.

035.

5. The method for preparing the PtPdRuCuBi high entropy alloy electrocatalyst for fuel cells according to claim 4, characterized in that: The mass ratio of P123, K2PtCl6, K2PdCl4, CuCl2, RuCl2·H2O-x, and BiN3O9·5H2O is approximately 1: 0.005-0.035: 0.005-0.035: 0.005-0.035: 0.005-0.035: 0.01-0.

030.

6. The method for preparing the PtPdRuCuBi high entropy alloy electrocatalyst for fuel cells according to claim 3, characterized in that: The heating reflux reaction temperature in step (1) is 200-230°C.

7. Use of the PtPdRuCuBi high entropy alloy electrocatalyst for fuel cells as claimed in claim 1 or 2 in electrocatalysis of ethanol.