Pressure-regulating casting gating system and method
By optimizing the design of the second straight runner and cross runner in the die-regulating casting system, the filling and replenishment of large and complex thin-wall receiver high-temperature alloy castings is achieved without increasing the filling and boosting speed. The shrinkage capability solves the problems of reverse filling and mold shell fire running, and significantly reduces casting defects and equipment requirements.
Patent Information
- Application Number
- CN202411045144.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-01
AI Technical Summary
The prior art is difficult to improve the filling and replenishment capabilities of large and complex thin-wall receiver high-temperature alloy castings without increasing the filling and boosting speed. Especially under the conditions of reverse gravity casting, reverse filling and molding are prone to occur. shell fire running and other issues.
A die-regulating casting casting system is designed, and the confluence position of the metal liquid is controlled by setting a first straight runner and a lower horizontal runner at the lower part of the mold, and the second straight runner is arranged on the upper part of the mold to connect with the upper horizontal runner. The filling capacity is used to fill the upper end and lower end to the middle simultaneously using a mixed casting method, and the inner diameter of the second runner is optimized to reduce filling time and defects.
It significantly improves the filling and shrinking capabilities of large and complex thin-wall receivers, reduces the defects of castings, reduces the quality requirements for equipment and mold shells, and achieves high-quality casting.
Smart Images

Figure CN118950942A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-temperature alloy precision casting, and in particular to a pressure-regulated casting pouring system and method. Background Art
[0002] As the structure of key hot-end components of aircraft engines develops towards large-scale, integrated and thin-walled, the difficulty of filling the mold caused by large size effect, variable cross-section effect and thin-wall effect during the forming and solidification process of large and complex thin-walled castings has gradually exceeded the limit of traditional gravity casting. As a kind of anti-gravity, pressure-regulated casting overcomes the limitations of traditional gravity casting of thin-walled castings and greatly improves the filling capacity and mechanical properties of thin-walled castings. As the factor with the greatest impact on the quality of castings in the casting process, the gating system has rarely been reported on the gating system for producing large and complex thin-walled castings such as casings under pressure-regulated casting.
[0003] In addition, in the process of pressure-regulated precision casting of large, complex, thin-walled castings such as casings using high-temperature alloys, in order to avoid defects such as insufficient pouring and cold shut, the method of increasing the filling and boosting speed is generally adopted to obtain a faster filling speed, thereby greatly improving the filling capacity. However, objectively, the selection of the filling and boosting speed is also restricted by objective conditions such as equipment and mold shell quality. The further increase in the filling and boosting speed will also place higher requirements on the equipment; and when the filling and boosting speed is high, it will also pose a great challenge to the quality of the mold shell, making it prone to problems such as mold shell fire, and there has been no good solution so far.
[0004] After searching, the Chinese invention patent with application publication number CN115283622A discloses a large-scale complex annular thin-walled casing mixed injection pouring system and pouring method, which can sequentially fill the castings, reduce the probability of undercasting, air entrapment, shrinkage and shrinkage holes in the castings, and improve the forming quality. However, the focus of this method is that the pouring system is only designed for conventional gravity casting, and it is not applicable to the pouring system of pressure-regulated casting. Moreover, it focuses on solving the shrinkage compensation problem of the hot joint of thin-walled castings, and does not explain the improvement of filling capacity.
[0005] The Chinese invention patent with application publication number CN114653924A discloses a low-pressure casting pouring system suitable for shrinkage compensation of complex thin-walled castings. The invention solves the problem of difficult arrangement of casting pouring systems, so that aluminum alloy castings with complex geometric shapes and thin walls have more shrinkage compensation channels and shorter shrinkage compensation paths during the casting process. However, in the process of anti-gravity casting, the metal liquid is easily filled from bottom to top under the action of pressure difference, and for high-temperature alloys with higher density than aluminum alloys, this reverse filling will have a greater impact on the quality of castings due to the increase in deadweight. In addition, there are differences between pressure-regulated casting and low-pressure casting. During the filling process of pressure-regulated casting, the reverse pressure in the mold shell is lower, and the resistance encountered by the metal liquid during the filling process is smaller. During the filling process of low-pressure casting, there is a certain reverse pressure in the mold cavity, which leads to certain limitations of this invention for the filling of complex thin walls of pressure-regulated casting high-temperature alloys.
[0006] In summary, there is an urgent need to design a pressure-regulated casting pouring scheme for casing castings, so as to improve the filling and shrinkage compensation capabilities of large, complex, thin-walled casing high-temperature alloy castings without increasing the filling and pressure increase speed. Summary of the invention
[0007] The purpose of the present invention is to provide a pressure-regulated casting pouring system and method to solve the problems existing in the above-mentioned prior art, and to improve the filling and shrinkage compensation capabilities of large, complex, thin-walled casing high-temperature alloy castings without increasing the filling and pressure-raising speed.
[0008] To achieve the above object, the present invention provides the following solutions:
[0009] The present invention provides a pressure-regulated casting pouring system, comprising: a first straight runner arranged at the lower part of the mold, the first straight runner being connected to a lower annular cross runner through a lower cross runner; a second straight runner arranged at the upper part of the mold, the second straight runner being coaxial with the first straight runner, and the second straight runner being connected to the lower cross runner; the second straight runner being connected to an upper annular cross runner and an upper end of an outer ring through an upper first cross runner; an inner gate at the lower end of the outer ring, located at the outer ring position of the casting, one end of the inner gate at the lower end of the inner ring being connected to the lower annular cross runner, and the other end of the inner gate being connected to the bottom of the inner ring of the casting; the second straight runner being connected to the upper end of the inner ring of the casting through an upper second cross runner.
[0010] The present invention establishes a three-dimensional solid model according to the structure of the casing casting. The overall structure of the casting is relatively complex. The casting is a double-ring structure with a large number of variable cross-section structures, large-area thin-walled areas concentrated at the inner and outer rings and the hollow support plates, and flange structures above and below the inner and outer rings. The casting as a whole is highly rotationally symmetrical. The areas of various parts of the casting system are calculated, the type of casting system and the pressurization speed are selected, and a traditional pressure-regulated casting system is established. Then, by controlling the inner diameter of the second straight runner, it is achieved to control the metal liquid convergence position and enhance the filling capacity without increasing the pressurization speed.
[0011] According to the casting material and casting structure, the pouring system type is selected, and the cross-sectional area ratio and number of the pouring system's sprue, cross runner and ingates are determined to establish a traditional pressure-regulated casting pouring system.
[0012] Optionally, the diameter of the second sprue is 20 mm.
[0013] Optionally, the diameter of the second sprue is 40 mm.
[0014] Optionally, the diameter of the second sprue is 70 mm. After assembling the pouring system and the casting, import them into the ProCAST numerical simulation software, and perform numerical simulation on the filling and solidification process of the castings with different second sprues for comparison. By numerically simulating the filling process of large and complex thin-walled castings, the fluid analysis module of the ProCAST software can simulate all the effects of liquid and solid flow, including filling, and couple the fluid flow and heat transfer through the complete Navier-Stocks flow equation. According to the simulation results of the above three-dimensional model, the filling time curves and shrinkage and shrinkage curves of different pouring systems are made at the same boost speed.
[0015] Optionally, the inner gate is set at the thick part of the casting, which is conducive to solidification shrinkage compensation and reduces casting defects. In addition, under pressure-regulated casting, the size of the inner gate also determines whether the metal liquid is filled by jet flow filling or uniform flow filling. The jet flow is prone to shrinkage defects, but can improve the filling of the casting to a certain extent. According to the structure of the casting, the product of the shrinkage compensation efficiency of the pressure-regulated casting gating system and the volume of the pressure-regulated casting gating system is greater than the overall shrinkage degree of the casting and the pressure-regulated casting gating system. The relationship is:
[0016] η×v1>ε×(v2+v1)
[0017] Among them, η is the shrinkage compensation efficiency of the pressure-regulated casting pouring system; ε is the volume shrinkage rate of the alloy; v1 is the volume of the pressure-regulated casting pouring system; v2 is the volume of the casting, and the alloy is a high-temperature alloy solution used for casting.
[0018] Optionally, since the high-temperature alloy is an easily oxidizable metal, the pouring system is set as an open pouring system, so that the metal liquid flow rate entering the mold cavity is small, the filling is smooth, and the metal oxidation is prevented. At the same time, the pouring system can provide sufficient filling metal, and the sum of the cross-sectional areas of the ingates is greater than the sum of the cross-sectional areas of the lower cross runner, the upper first cross runner and the upper second cross runner. The sum of the cross-sectional areas of the lower cross runner, the upper first cross runner and the upper second cross runner is greater than the sum of the cross-sectional areas of the first straight runner and the second straight runner, which satisfies the relationship, ∑A ingates>∑A cross runner>∑A straight runner. In the casting process, the ingates refer to the channel for transporting molten metal from the straight runner or the cross runner to the casting cavity, which belongs to the prior art. It is a key component of the pouring system, responsible for accurately and effectively introducing the molten metal from the main gate to various parts of the mold to ensure uniform filling and good molding of the casting.
[0019] Optionally, according to the relevant theory of casting filling, a relatively slow filling speed should be used for thick-walled and simple-structured castings, and a relatively fast filling speed should be selected for thin-walled and complex castings. In the present invention, for complex thin-walled castings such as large casings, the filling pressure increase speed is 15kPa / s. According to the Bernoulli equation, the relationship between the pressure increase speed and the filling speed during pouring is:
[0020]
[0021] Where, P(t)-pressurization speed, t-filling time, ρ-alloy density, g-gravitational acceleration, V-metal liquid filling speed, metal liquid is alloy metal liquid, A f - Riser cross-sectional area, A F - Cross-sectional area of the crucible used for casting.
[0022] Optionally, according to the casting structure and the three-dimensional model of the traditional pressure-regulated casting pouring system, it is imported into the ProCAST numerical simulation software according to the determined pouring assembly method, and the filling and solidification process of the casting of the traditional pouring system is numerically simulated. Based on the design method of the mixed pouring system in the gravity casting method. The three-dimensional model of the traditional pressure-regulated casting system is optimized. In order to enhance filling and shrinkage compensation, the upper runner of the casing casting is added, and the size of the second straight runner is controlled to control the filling time and shrinkage cavities. The shrinkage cavity content of large and complex thin-walled castings after solidification is calculated by numerical simulation. The ProCAST software uses the Niyama criterion (Ny). The Niyama criterion and ProCAST software are both prior arts. The Niyama criterion is widely used in investment casting. The criterion for judging the shrinkage cavity content of the casting after solidification by the Niyama criterion is as follows:
[0023]
[0024] Where G is the temperature gradient and T is the cooling rate.
[0025] The present invention also provides a pressure-regulated casting pouring method, comprising the following steps:
[0026] Design the inner diameter of the second sprue;
[0027] Select the pressurization speed according to the wall thickness and structure of the casting;
[0028] The second sprue is used to divert the molten metal, and the casting is simultaneously filled from the upper end and the lower end to the middle by a mixed pouring method to achieve the casting of the casting.
[0029] Compared with the prior art, the present invention has achieved the following technical effects:
[0030] The present invention optimizes the traditional pressure-regulated casting pouring system without changing the pressure-regulated casting boosting speed, and controls the time required for filling and the position of the molten metal confluence by controlling the size of the second straight runner of the optimized pouring system, and significantly reduces casting defects. On the one hand, the present invention adopts a second straight runner to connect the lower cross runner to divert the molten metal, and the casting is simultaneously filled from the upper end and the lower end to the middle in a mixed pouring method, thereby shortening the overall filling time of the casting and reducing the tendency of undercasting, and the position of the alloy liquid confluence in the casting can be controlled by controlling the size of the center column; the filling time can be controlled by controlling the size of the center column, and its filling capacity can be enhanced at a certain boosting speed, reducing the requirements for equipment and mold shell quality. On the other hand, risers are provided at the upper and lower ends of the casting, and the risers are fully connected to the pouring system to form an annular structure, which ensures the shrinkage compensation of the casting, and can effectively transfer the thermal stress of the casting to the pouring system to prevent the casting from excessive thermal deformation. Based on the above design, high-quality casting of large-sized complex annular thin-walled casings is achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0032] Figure 1 It is a structural schematic diagram of a casting and a pressure-regulated casting pouring system in the prior art;
[0033] Figure 2 It is a structural schematic diagram of a casting and a pressure-regulated casting pouring system in the prior art from another angle;
[0034] Figure 3 for Figure 1A cross-sectional view of
[0035] Figure 4 A schematic diagram of the structure of a casting and a pouring system according to an embodiment of the present invention;
[0036] Figure 5 for Figure 4 Schematic diagram from another angle;
[0037] Figure 6 for Figure 4 A cross-sectional view of
[0038] Figure 7 A schematic structural diagram of a casting and a pouring system according to another embodiment of the present invention;
[0039] Figure 8 for Figure 7 Schematic diagram from another angle;
[0040] Fig. 9 for Figure 7 A cross-sectional view of
[0041] Fig.10 A schematic structural diagram of a casting and a pouring system according to a third embodiment of the present invention;
[0042] Fig.11 for Fig.10 Schematic diagram from another angle;
[0043] Fig.12 for Fig.10 sectional view of
[0044] Fig.13 It is a schematic diagram comparing the time required for filling the mold cavity by the pouring system in the prior art and the pouring system of the present invention;
[0045] Fig.14 It is a schematic diagram comparing the shrinkage porosity content after solidification between the gating system in the prior art and the gating system of the present invention;
[0046] In the figure: 1-casting, 2-pouring system, 3-first straight runner, 4-lower runner, 5-lower annular runner, 6-ingate at the lower end of the outer ring, 7-ingate at the lower end of the inner ring, 8-second straight runner, 9-upper first runner, 10-upper second runner, 11-upper annular runner. DETAILED DESCRIPTION
[0047] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0048] The purpose of the present invention is to provide a pressure-regulated casting pouring system and method to solve the problems existing in the above-mentioned prior art, and to improve the filling and shrinkage compensation capabilities of large, complex, thin-walled casing high-temperature alloy castings without increasing the filling and pressure-raising speed.
[0049] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0050] The present invention provides a pressure regulating casting pouring system, such as Figure 1 , Figure 2 , Figure 3 As shown, it is the structure of the existing pouring system, which includes a casting 1 and a pouring system 2 for pouring high-temperature alloy molten metal. The casting 1 is a large and complex thin-walled casing casting. The overall structure of the thin-walled casing casting is relatively complex. It is a highly rotationally symmetrical double-ring structure consisting of an inner ring, an outer ring and a hollow support plate. There are a large number of variable-section structures and large-area thin-walled areas on it. The main structure of the traditional pressure-regulated casting pouring system for pouring high-temperature alloy molten metal includes: a first straight runner 3, a lower cross runner 4, a lower annular cross runner 5, an inner gate 6 at the lower end of the outer ring, and an inner gate 7 at the lower end of the inner ring.
[0051] like Figure 4 , Figure 5 , Figure 6 As shown, the structure of an embodiment of the present invention includes a large complex thin-walled casing casting 1 and a modified and optimized pouring system 3 for pouring high-temperature alloy molten metal. The pouring system structure mainly includes: a first straight runner 3, a lower cross runner 4, a lower annular cross runner 5, an inner gate at the lower end of the outer ring 6, an inner gate at the lower end of the inner ring 7, a second straight runner 8, the second straight runner 8 has a diameter of 20 mm, an upper first cross runner 9, an upper second cross runner 10, and an upper annular cross runner 11.
[0052] like Figure 7 , Figure 8 , Fig. 9 As shown, in another specific embodiment, the diameter of the second sprue 8 is 40 mm.
[0053] like Fig.10 , Fig.11 , Fig.12 As shown, in the third specific embodiment, the diameter of the second sprue 8 is 70 mm.
[0054] According to the casting material and casting structure, the type of pouring system is selected, and the cross-sectional area ratio and number of the pouring system's sprue, cross runner and ingode are determined to establish a traditional pressure-regulated casting pouring system. The ingode (the contact surface between the ingode and the casting) is located at a thicker part of the casting wall, which is helpful for solidification shrinkage compensation and suppressing casting defects. Under pressure-regulated casting, the ingode includes the ingode 6 at the lower end of the outer ring and the ingode 7 at the lower end of the inner ring. The size of the ingode also determines whether the metal liquid is filled by injection, and injection is prone to casting defects. According to the casting structure, the product of the shrinkage compensation efficiency of the pressure-regulated casting pouring system and the volume of the pressure-regulated casting pouring system is greater than the overall shrinkage of the casting and the pressure-regulated casting pouring system. The relationship is: η×v1>ε×(v2+v1)
[0055] Where:
[0056] η is the shrinkage-compensation efficiency of the pressure-regulated casting pouring system; ε is the volume shrinkage rate of the alloy; v1 is the volume of the pressure-regulated casting pouring system; v2 is the volume of the casting.
[0057] Since the high-temperature alloy is an easily oxidized metal, the pouring system is set as an open pouring system, so that the metal liquid flow rate entering the cavity is small, the filling is smooth, and the oxidation of the high-temperature alloy metal liquid is prevented. At the same time, the pouring system can provide sufficient filling metal. The sum of the cross-sectional areas of the ingates is greater than the sum of the cross-sectional areas of the lower cross runner, the upper first cross runner and the upper second cross runner, and the sum of the cross-sectional areas of the lower cross runner, the upper first cross runner and the upper second cross runner is greater than the sum of the cross-sectional areas of the first straight runner and the second straight runner, which satisfies the relationship, ∑A ingates>∑A cross runner>∑A straight runner.
[0058] According to the relevant theories of casting filling, a relatively slow filling speed should be adopted for thick-walled and simple-structured castings, and a relatively fast filling speed should be selected for thin-walled complex castings. The large casing-type complex thin-walled castings involved in this embodiment are very likely to cause defects such as insufficient pouring and cold shut for large thin-walled castings filled with high-temperature alloys. However, when the filling pressure boosting speed is high, the quality of the mold shell is difficult to meet the requirements at this stage. Therefore, in the embodiment of the present invention, based on actual conditions, the filling pressure boosting speed is 15kPa / s. Under pressure-regulated casting, the present invention can reduce the filling time and reduce shrinkage and shrinkage holes by controlling the second straight runner at a boosting speed of 15kPa / s, and can even control the position of the metal liquid converging in the casting by controlling the diameter of the second straight runner, so as to avoid converging at important positions and enhance the filling capacity. By optimizing the pouring system and changing the diameter of the second straight runner of the optimized pouring system, the filling capacity and shrinkage compensation capacity of the casting can be improved without increasing the pressurization speed.
[0059] According to the Bernoulli equation, the relationship between pressurization speed and filling speed can be calculated as follows:
[0060]
[0061] In the formula, P(t)-pressurization speed, t-filling time, ρ-alloy density, g-gravitational acceleration, V-metal liquid filling speed, A f - Riser cross-sectional area, A F - Cross-sectional area of the crucible.
[0062] Taking the design of K4800 nickel-based high-temperature alloy anti-gravity pressure-regulated precision casting pouring system as an example, the technical solution of this application is further explained in detail. Different pressure-raising speeds of molten metal in pressure-regulated casting also have different effects on the diameter of the second sprue of the pouring system. When the pressure-raising speed is lower than 5kPa / s, the filling time does not decrease with the increase of the diameter of the second sprue, and the filling time is increased compared with the traditional design method; when the pressure-raising speed is higher than 30kPa / s, a smaller diameter of the second sprue can reduce the filling time, but in general, the filling time can be regulated by controlling the second sprue. In actual use, there is no specific restriction on the filling pressure-raising speed, and the appropriate value can be selected as needed.
[0063] The design method in this embodiment is applicable to large-sized complex thin-walled casing castings.
[0064] Figure 1 , Figure 2 , Figure 3 It is a schematic diagram of the traditional pressure-regulated casting pouring system and assembly structure.
[0065] The present invention optimizes the traditional pressure-regulated casting pouring system and adds filling and shrinkage-compensating runners to the upper part of the casting. At the same time, the second straight runner 8 is controlled to be 20mm, 40mm, and 70mm respectively to control its filling process and the required time. Some specific parameters involved in the simulation verification process are as follows: The filling and pressure increase speed is selected to be 15kpa / s. The outer ring wall diameter of casting 1 is 328mm, the inner ring wall diameter of casting 1 is 168mm, and the overall height of the casting is 105mm.
[0066] Statistics on the time required for complete filling of castings under different gating systems, such as Fig.13As shown. It can be found that the alloy liquid completely fills the cavity. For the traditional pouring system, the filling time is relatively low, which is 1.53s, but the casting has many defects such as shrinkage and shrinkage holes. For the optimized and improved pouring system No. 1, due to the increase in the volume of the pouring system, more molten metal is required to fill the mold, so the required filling time increases to 2.84s, but the defects such as shrinkage and shrinkage holes of the casting are greatly reduced; the size of the second straight runner is further expanded to 40mm, and this is the improved pouring system No. 2. Its filling time is sharply reduced compared with the pouring system with a second straight runner size of 20mm, and it is not much different from the traditional pouring system, which is 1.67s; on this basis, the size of the second straight runner is further increased to 70mm, and this is the improved pouring system No. 3, and its filling time is the fastest compared with the previous ones, which is 1.31s. It can be found that at the same filling and pressure rise speed, with the increase of the size of the second straight runner, the time required to complete the filling is significantly reduced. Therefore, the filling speed of large and complex thin-walled casing castings can be controlled by controlling the size of the second straight runner of the optimized pressure-regulated casting gating system, and the simulation results show that it can also control the convergence position of the molten metal.
[0067] In addition, the shrinkage and shrinkage defects that appear after the castings are filled and solidified under different gating systems are statistically analyzed, such as Fig.14 It can be found that, on the one hand, the optimized gating system has significantly reduced shrinkage and shrinkage cavity content compared with the gating system before optimization, which improves the quality of castings; on the other hand, the defect content between the gating systems of the second straight runners of different sizes is not much different, and simply presents a trend of increasing first and then decreasing.
[0068] In summary, the modified design method of the pouring system in the embodiment of the present invention has well solved the shortcomings of the traditional design method. For large-sized, complex, thin-walled casing castings, the pouring system designed using the method of the embodiment of the present invention can make the metal liquid fill the mold quickly while significantly reducing casting defects.
[0069] The above embodiment is illustrated by taking the design of the precision casting pouring system for counter-gravity pressure-regulated casting as an example. On the basis of the design of the traditional precision casting pouring system for counter-gravity casting, the traditional pouring system for pressure-regulated casting is optimized according to the design method of the mixed-injection pouring system in the gravity casting method. By adjusting the size of the second straight runner of the optimized pouring system, the purpose of controlling the operation and controllability of large-sized, complex, thin-walled casing castings is achieved.
[0070] The pouring system design method in the embodiment of the present invention is applicable to anti-gravity casting processes such as low-pressure casting, differential pressure casting and pressure-regulated casting; and can be used for different casting materials such as cast iron, cast steel, aluminum alloy, magnesium alloy, copper alloy, titanium alloy, nickel-based high-temperature alloy, etc. The pouring system design method in the above embodiment can more reasonably improve the filling capacity of the casting and provide the casting forming quality without increasing the filling pressure increase speed.
[0071] The present invention uses specific examples to illustrate the principles and implementation methods of the present invention. The above examples are only used to help understand the method and core ideas of the present invention. At the same time, for those skilled in the art, according to the ideas of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A pressure regulating casting pouring system, characterized in that: include: A first sprue is provided at the lower part of the mold, wherein the first sprue is connected to a lower annular runner through a lower runner; A second sprue is arranged at the upper part of the mold, the second sprue is coaxial with the first sprue, and the second sprue is connected with the lower runner; the second sprue is connected with the upper annular runner and the upper end of the outer ring of the casting through the upper first runner; The inner gate at the lower end of the outer ring is located at the outer ring position of the casting, one end of which is connected to the lower annular runner, and the other end of which is connected to the bottom of the outer ring of the casting; The inner gate at the lower end of the inner ring is located at the inner ring position of the casting, one end of the inner gate at the lower end of the inner ring is connected to the lower cross runner, and the other end is connected to the bottom of the inner ring of the casting; The second sprue is connected to the upper end of the inner ring of the casting through the upper second cross runner.
2. The pressure-regulated casting pouring system according to claim 1, characterized in that: The diameter of the second sprue is 20 mm.
3. The pressure-regulated casting pouring system according to claim 1, characterized in that: The diameter of the second sprue is 40 mm.
4. The pressure-regulated casting pouring system according to claim 1, characterized in that: The diameter of the second sprue is 70 mm.
5. The pressure-regulated casting pouring system according to claim 1, characterized in that: The product of the shrinkage compensation efficiency of the pressure-regulated casting gating system and the volume of the pressure-regulated casting gating system is greater than the overall shrinkage of the casting and the pressure-regulated casting gating system. The relationship is: η×v1>ε×(v2+v1) Among them, η is the shrinkage compensation efficiency of the pressure-regulated casting pouring system; ε is the volume shrinkage rate of the alloy; v1 is the volume of the pressure-regulated casting pouring system; v2 is the volume of the casting.
6. The pressure-regulated casting pouring system according to claim 1, characterized in that: The sum of the cross-sectional areas of the ingates is greater than the sum of the cross-sectional areas of the lower runner, the upper first runner and the upper second runner, and the sum of the cross-sectional areas of the lower runner, the upper first runner and the upper second runner is greater than the sum of the cross-sectional areas of the first straight runner and the second straight runner, which satisfies the relationship, ∑A ingates > ∑A runner > ∑A straight runner.
7. The pressure-regulated casting pouring system according to claim 1, characterized in that: The relationship between the pressure increase speed and the filling speed during pouring is: In the formula, P(t)-pressurization speed, t-filling time, ρ-alloy density, g-gravitational acceleration, V-metal liquid filling speed, A f - Riser cross-sectional area, A F - Cross-sectional area of the crucible.
8. The pressure-regulated casting pouring system according to claim 1, characterized in that: The Niyama criterion is used to determine the shrinkage porosity content of the casting after solidification. The criterion is: Where G is the temperature gradient and T is the cooling rate.
9. The pressure regulating casting pouring method of the pressure regulating casting pouring system according to any one of claims 1 to 8, characterized in that: The steps include: Design the inner diameter of the second sprue; Select the pressurization speed according to the wall thickness and structure of the casting; The second sprue is used to divert the molten metal, and the casting is simultaneously filled from the upper end and the lower end to the middle by a mixed pouring method to achieve the casting of the casting.
Citation Information
Patent Citations
High-temperature alloy large-scale cartridge receiver casting bottom-filling type pouring system and pouring method
CN111922290A
Large-size complex annular thin-wall casing mixed injection type pouring system and pouring method
CN115283622A
Design method of casting and pouring system for variable-cross-section thin-wall casting
CN116921627A
Cited By
Device for testing forming quality of pressure-regulating cast high-temperature alloy thin wall
CN120028509A
A testing device for the forming quality of thin-walled superalloy in pressure regulating casting
CN120028509B
Anti-gravity pressure regulating precision casting pouring system for front diffuser casing
CN120079808A
A front diffuser casing counter-gravity pressure regulating precision casting pouring system
CN120079808B
Variable-cross-section high-temperature alloy casting and machining method and application thereof
CN120791348A