By using a variety of alloy elements and advanced processes such as RH vacuum degassing and carburizing treatment in the hot rolling process of high-strength steel, the microstructure of the steel is optimized, and the problem of insufficient corrosion resistance and fatigue resistance in traditional processes is solved. , significantly improves the performance of steel.
Patent Information
- Application Number
- CN202411100137.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-15
AI Technical Summary
The traditional hot-rolling preparation process of high-strength steel has room for improvement in corrosion resistance and fatigue resistance. The raw material ratio is single, and the synergy of multiple alloy elements has been failed to fully utilize.
Using the synergistic effect of a variety of alloy elements such as silicon, manganese, chromium, nickel, molybdenum, titanium, cerium, vanadium, etc., through the smelting process of blast furnace and steelmaking electric furnace, combined with RH vacuum degassing method and carburizing treatment, finishing rolling and Multi-stage cooling process optimizes the microstructure and performance of steel.
It significantly improves the hardness, wear resistance and fatigue resistance of steel, extends the service life, and improves the reliability and safety of the equipment.
Smart Images

Figure CN118957412A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of steel preparation, and in particular relates to a high-strength steel hot rolling preparation process. Background Art
[0002] High-strength steel has become a high-quality steel due to its high strength, high toughness, high heat resistance and high corrosion resistance. Compared with traditional steel, high-strength steel has higher yield strength and tensile strength, and can withstand greater loads and pressures. In the field of steel preparation technology, high-strength steel, as an important metal material, is widely used in shipbuilding. In view of the working environment of the ship, steel has to withstand a variety of dynamic and irregular loads such as erosion from seawater, wind, ship movement and waves, and has high requirements for the corrosion resistance and fatigue resistance of steel. However, the high-strength steel prepared by the traditional high-strength steel preparation process still has room for improvement in corrosion resistance and fatigue resistance. Specifically, the traditional high-strength steel hot rolling preparation process is often relatively simple in the raw material ratio, and fails to fully utilize the synergistic effect of multiple alloying elements to improve the performance of steel. In this regard, we propose a high-strength steel hot rolling preparation process. Summary of the Invention
[0003] In view of the deficiencies in the prior art, the present invention provides a high-strength steel hot rolling preparation process to solve the above technical problems.
[0004] To achieve the above-mentioned object, the present invention provides the following technical solution: a high-strength steel hot rolling preparation process, the high-strength steel hot rolling preparation process steps are: S1. Prepare the following raw materials: 500-2000 parts of iron ore, 400-600 parts of coke, 300-500 parts of limestone, 125-500 parts of silicon, 100-500 parts of manganese, 50-300 parts of chromium, 50-200 parts of nickel, 10-100 parts of molybdenum, 10-50 parts of titanium, 5-50 parts of cerium, 10-100 parts of vanadium, 200-500 parts of desulfurizer, and 200-500 parts of dephosphorizer. S2, putting the iron ore into the crusher for crushing; S3, placing iron ore, coke and limestone in a blast furnace until blast furnace gas and liquid iron are produced, and adding a desulfurizer and a dephosphorization agent; S4, adding blast furnace pig iron and silicon, silicon, manganese, chromium, nickel, molybdenum, titanium, cerium and vanadium into a steelmaking electric furnace for heating and smelting, and adding desulfurizer and desulfurizer again; S5. The refined molten steel is sent to the LF refining furnace, and the inclusions and gases in the molten steel are removed by RH vacuum degassing; S6. The refined molten steel is continuously cast into billets, and the continuously cast billets are sent to a heating furnace to eliminate internal stress; S7, the steel billet is sent to the roughing mill for initial rolling to form a primary shape, and then sent to the intermediate rolling mill for further rolling, and then finished rolling is carried out under high temperature and high pressure; S8. After finishing rolling, the steel is rapidly cooled by water cooling and then quality tested.
[0005] Preferably, the high-strength steel is specifically composed of the following components: 1080 parts of iron ore, 350 parts of coke, 320 parts of limestone, 270 parts of silicon, 288 parts of manganese, 180 parts of chromium, 120 parts of nickel, 45 parts of molybdenum, 40 parts of titanium, 27 parts of cerium, 64 parts of vanadium, 210 parts of desulfurizer, and 230 parts of dephosphorizer.
[0006] Preferably, in step S3, the heating temperature of the blast furnace is 1200° C.-1500° C., and the heating and melting time is 4 hours.
[0007] Preferably, the timing of adding the alloying elements in step S4 is: A1. Silicon is added at the beginning of the reduction period. Wait 10 minutes after adding it to ensure that the ferrosilicon is completely melted. A2. Manganese is added after the slagging and carbonization operations are completed; A3. Chromium is added at the beginning of the reduction period. After adding, the color of the slag needs to be observed. If it turns green, the reduction needs to be strengthened. A4. Nickel is added during the refining period; A5. Ferromolybdenum is added at the beginning of the reduction period; A6. Titanium is added in the late reduction period. Before adding, aluminum and titanium need to be added to the steel to deoxidize and stabilize nitrogen; A7. Cerium is added during the refining period; A8. Vanadium is added after the slag and molten steel are well deoxidized during the reduction period.
[0008] Preferably, the RH vacuum degassing method in step S5 is as follows: insert the two immersion tubes at the lower part of the vacuum chamber into the molten steel, start the vacuum pump, evacuate the vacuum chamber, blow argon gas from about one-third of the lower part of the riser, and the gas in the molten steel is rapidly precipitated under the action of the vacuum and is pumped away by the vacuum pump. The degassed molten steel is collected at the bottom of the vacuum chamber, and the undegassed molten steel enters the vacuum chamber from the riser and returns from the downcomer after degassing, forming a cycle. The number of cycles is 5, and the cycle time for each cycle is controlled within 3 minutes.
[0009] Preferably, in step S6, the continuous casting speed is controlled at 3.0-7.0 m / min, the heating temperature is controlled at 1200° C.-1300° C., and the heating time is 3.5 h-6 h.
[0010] Preferably, the quality inspection in step S8 includes appearance inspection, physical property test, metallographic structure inspection, non-destructive inspection and hardness inspection.
[0011] Preferably, the steel needs to be post-processed after the test is completed to improve the fatigue resistance of the steel.
[0012] Preferably, the post-processing steps are: B1. Heat the steel to 850℃-1000℃ to make the solid carburizing agent fully contact with the steel surface; B2. Keep at 900℃ for 1 hour to allow carbon atoms to penetrate into the steel surface; B3. After carburizing is completed, the steel is taken out from the solid carburizing agent and cooled using a multi-stage cooling method.
[0013] Preferably, the multi-stage cooling method is divided into three stages. The first stage uses water cooling to reduce the steel temperature to 500℃~550℃ for 20 minutes. The second stage uses air cooling to reduce the steel temperature to 200℃~250℃ for 1 hour. The third stage uses natural cooling to room temperature for 3 hours.
[0014] Compared with the prior art, the present invention has the following beneficial effects: This application improves the hardness and wear resistance of steel through the process of preparing high-strength steel and the alloying elements added during the preparation, and significantly improves the corrosion resistance and fatigue resistance of steel. The carburizing treatment process improves the hardness and wear resistance of steel, so that the treated steel performs well in application scenarios requiring high hardness and wear resistance. The multi-stage cooling method effectively controls the cooling rate of steel, reduces the thermal stress and deformation caused by rapid cooling, thereby ensuring the dimensional stability and processing performance of steel. The microstructure of steel is optimized and the grains are refined, which improves the fatigue resistance of steel. This is especially important for components that need to withstand alternating loads, and can extend their service life and improve the reliability and safety of the overall equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is the process flow chart of hot rolling preparation of high-strength steel. DETAILED DESCRIPTION
[0016] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0017] The present invention provides a technical solution: a high-strength steel hot rolling preparation process, the high-strength steel hot rolling preparation process steps are: S1. Prepare the following raw materials: 500-2000 parts of iron ore, 400-600 parts of coke, 300-500 parts of limestone, 125-500 parts of silicon, 100-500 parts of manganese, 50-300 parts of chromium, 50-200 parts of nickel, 10-100 parts of molybdenum, 10-50 parts of titanium, 5-50 parts of cerium, 10-100 parts of vanadium, 200-500 parts of desulfurizer, and 200-500 parts of dephosphorizer. S2. Place the iron ore into the crusher for crushing. The crushing method is multi-stage crushing to ensure uniform particle size, improve the permeability of the blast furnace charge column, and reduce energy consumption; S3, iron ore, coke and limestone are placed in a blast furnace until blast furnace gas and liquid iron are produced, the high temperature generated by the combustion of coke is used to reduce the iron oxide in the iron ore, while the limestone is decomposed to form alkaline slag, which removes harmful elements in the molten iron, and desulfurizers and dephosphorizers are added to reduce the sulfur and phosphorus content in the molten iron; S4, adding blast furnace pig iron and silicon, silicon, manganese, chromium, nickel, molybdenum, titanium, cerium and vanadium into a steelmaking electric furnace for heating and smelting using electric energy, controlling the chemical composition and temperature of the molten steel through electromagnetic stirring and oxygen blowing decarburization process, adding desulfurizer and desulfurizer again to further reduce the sulfur and phosphorus contents in the molten steel, and controlling the phosphorus and sulfur contents to below 0.005% and 0.002%, respectively; S5. The refined molten steel is fed into the LF refining furnace, where refined slag is added, and the temperature and time are adjusted to remove inclusions and gases in the molten steel. The hydrogen and nitrogen gases in the molten steel are quickly removed under vacuum conditions by the RH vacuum degassing method to improve the intrinsic quality of the steel. S6. The refined molten steel is rapidly cooled and solidified by a continuous casting machine and continuously cast into a billet, which is then sent to a heating furnace to eliminate internal stress. S7. The steel billet is sent to the roughing mill for initial rolling to form a primary shape. After rough rolling, the steel billet is sent to the intermediate rolling mill for further rolling to refine the grains and improve the density and mechanical properties of the steel. Finish rolling is then carried out under high temperature and high pressure. The rolling speed and reduction are precisely controlled to ensure the dimensional accuracy and surface quality of the steel. S8. After finish rolling, the steel is rapidly cooled by water cooling to fix the structure and properties after rolling, and then quality inspection is carried out to ensure that each batch of steel meets the standards of high strength, high toughness and high corrosion resistance.
[0018] Furthermore, the high-strength steel is specifically composed of the following ingredients: 1080 parts of iron ore, 350 parts of coke, 320 parts of limestone, 270 parts of silicon, 288 parts of manganese, 180 parts of chromium, 120 parts of nickel, 45 parts of molybdenum, 40 parts of titanium, 27 parts of cerium, 64 parts of vanadium, 210 parts of desulfurizer, and 230 parts of dephosphorizer.
[0019] Furthermore, the heating temperature of the blast furnace in step S3 is 1200℃-1500℃. Within this temperature range, the coke can be fully burned to generate high temperature to reduce the iron oxide in the iron ore and maintain the air permeability in the blast furnace. Too high a temperature will accelerate the erosion of the blast furnace refractory materials and increase energy consumption. Too low a temperature will lead to incomplete reduction, affecting the output and quality of the molten iron. In order to ensure that the iron ore is fully reduced and melted, the heating and melting time is 4H. The physical and chemical changes that the iron ore undergoes during this period include evaporation of water, decomposition of carbonates, reduction and melting of iron. The heating time is precisely controlled to ensure that the iron element in the iron ore is reduced to the maximum extent, reduce the content of impurities and improve the purity of the molten iron.
[0020] Furthermore, the timing of adding alloying elements in step S4 is: A1. Silicon is mainly used for deoxidation and alloying in the steelmaking process. Silicon is added in the early stage of the reduction period because the oxygen content in the molten steel is high. Silicon can quickly combine with oxygen to form silicate, which is used to remove impurities and gases in the molten steel. After adding silicon, wait for 10 minutes to ensure that the ferrosilicon is completely melted to reduce the oxygen content in the molten steel. A2. Manganese is added after the slag removal and carbonization operation is completed. Manganese is an effective deoxidizer. It combines with sulfur in molten steel to form manganese sulfide, reducing the sulfur content in the molten steel. Adding manganese after slag removal avoids the rolling reaction between manganese and slag, improving the utilization rate of manganese. Adding manganese after carbonization will ensure the stability of the carbon content in the molten steel and help the alloying effect of manganese. A3. The addition of chromium can improve the corrosion resistance and hardness of steel. Chromium is added at the beginning of the reduction period because the molten steel temperature is higher at this time, which facilitates the melting and diffusion of chromium. After adding chromium, the color of the slag should be observed. If it turns green, it means that chromium has reacted with oxygen in the molten steel to form chromium oxide. At this time, it is necessary to strengthen the reduction to improve the chromium yield and reduce the formation of harmful impurities. A4. Nickel is mainly used to improve the strength and toughness of steel. Since nickel has a high melting point and easily combines with other elements in molten steel to form stable compounds, nickel is added during the refining stage. During this period, the temperature and chemical composition of the molten steel have stabilized, facilitating the uniform distribution of nickel and alloying. A5. Ferromolybdenum is an important alloying element that improves the high-temperature strength and corrosion resistance of steel. Ferromolybdenum is added at the beginning of the reduction period. Ferromolybdenum has a high melting point and high solubility in molten steel, and can quickly mix with the molten steel to exert its effect. A6. Titanium is added in the late reduction period. Before adding it, aluminum and titanium need to be added to the steel to deoxidize and stabilize nitrogen. Because titanium has a strong affinity, it easily combines with oxygen and nitrogen in the molten steel to form stable compounds. By pre-deoxidizing and stabilizing the nitrogen content, it is ensured that titanium exists in the molten steel in a single state, allowing it to play a role in strengthening and refining grains. A7. Cerium is a rare earth element that has the ability to purify molten steel, refine grains, and improve steel properties. Cerium is added during the refining stage. During the refining process, the chemical composition and temperature of the molten steel have been well controlled. At this time, adding cerium can fully play its role in purifying the molten steel and refining grains. A8. Vanadium is added after the slag and molten steel are well deoxidized during the reduction period. Vanadium can improve the strength and toughness of steel. Vanadium easily combines with oxygen in the molten steel to form oxides, which affects the alloying effect of vanadium. Adding vanadium after the slag and molten steel are well deoxidized can ensure that vanadium exists in the molten steel in a single state.
[0021] Furthermore, the RH vacuum degassing method in step S5 is as follows: insert the two immersion tubes at the bottom of the vacuum chamber into the molten steel, start the vacuum pump, and as the vacuum degree gradually increases, a negative pressure environment is formed in the vacuum chamber, creating favorable conditions for the subsequent molten steel degassing process. When the vacuum chamber is evacuated, argon is blown into the lower third of the riser. Argon is used as an inert gas to stir the molten steel and promote the precipitation of gas in the molten steel. The gas in the molten steel is rapidly precipitated under the action of vacuum and is pumped away by the vacuum pump. The degassed molten steel is collected at the bottom of the vacuum chamber, and the undegassed molten steel enters the vacuum chamber from the riser and returns from the downcomer after degassing, forming a cycle. The number of cycles is 5, and the cycle time for each cycle is controlled within 3 minutes to ensure degassing efficiency and avoid adverse effects caused by excessive treatment. When the preset number of cycles and time are reached, the argon blowing and the vacuum pump are stopped to end the degassing process. At this time, the gas content in the molten steel is greatly reduced, and the purity of the molten steel is significantly improved. The vacuum chamber is then separated from the ladle and cleaned and maintained for next use.
[0022] Furthermore, in step S6, the continuous casting speed is controlled at 3.0-7.0 m / min. Since the steel grade has good solidification, strong crystallizer cooling capacity, and stable equipment operation, a higher continuous casting speed is adopted to improve production efficiency. The heating temperature is controlled at 1200°C-1300°C. This temperature range can ensure that the steel billet is completely austenitized, reduce internal stress, improve deformation capacity during rolling, avoid overheating of the steel billet, and reduce the occurrence of grain coarsening and overburning. The heating time is 3.5h-6h.
[0023] Furthermore, the quality inspection in step S8 includes appearance inspection, physical property test, metallographic structure inspection, non-destructive testing and hardness test; Appearance inspection is a comprehensive inspection of the product's appearance using visual inspection and simple tools. It includes checking whether the product's dimensions meet the requirements of the drawings, whether the surface is flat and smooth, and whether there are cracks, slag inclusions, scratches, or rust. Appearance inspection aims to eliminate any external problems that may affect the product's aesthetics or subsequent performance. Physical performance testing is a key step in measuring whether a product's physical properties meet specified standards. It includes tensile testing, impact testing, and bending testing to evaluate key performance indicators such as strength, toughness, hardness, and ductility. Through testing, we understand the product's behavior under various stress conditions and ensure that it can withstand the expected loads and impacts during normal use. Metallographic testing is to observe the microstructure of the product through a microscope and analyze its grain size, morphology, distribution and phase composition. It is of great significance for understanding the mechanical properties, corrosion resistance and heat treatment effect of the product. Through metallographic testing, it is possible to evaluate whether the heat treatment process of the product is appropriate, whether there are any overheating, overburning or decarburization problems, and whether the expected microstructure state has been achieved. Non-destructive testing (NDT) is a method of inspecting the interior or surface of a product using the principles of sound, light, electricity, and magnetism without damaging its structure and performance. Common NDT techniques include ultrasonic testing, X-ray testing, magnetic particle testing, and penetrant testing. These techniques can effectively detect cracks, inclusions, and porosity within a product, as well as assess key indicators such as welding quality and material uniformity. NDT is crucial to ensuring product safety and reliability. Hardness testing is an indicator that measures a product's ability to resist local indentation deformation. It is also an important means of evaluating product material properties and heat treatment effects. Commonly used hardness testing methods include Brinell hardness testers, Rockwell hardness testers, and Vickers hardness testers. Through hardness testing, we can understand the hardness distribution of different parts of the product and the changes in hardness after heat treatment. Hardness testing is of great significance for determining the product's scope of use, processing performance, and predicting its wear and life during use.
[0024] Furthermore, after the inspection is completed, the steel needs to be post-processed to improve its fatigue resistance. Steel is prone to fatigue damage during long-term use, especially when subjected to repeated stress. Improving the fatigue resistance of steel means that the steel can withstand more cycles without damage under the same stress level, thereby significantly extending its service life.
[0025] Further, the post-processing steps are: B1. The steel is placed in a special carburizing furnace and heated to 850℃-1000℃. During the heating process, the surface of the steel begins to soften, preparing for the subsequent carburizing process and allowing the solid carburizing agent to fully contact the steel surface; B2. Maintain at 900°C for 1 hour to ensure that carbon atoms have enough time to diffuse from the carburizing agent to the surface of the steel and further penetrate into the interior through the grain boundaries and intragranular defects of the steel; B3. After carburizing is completed, the steel is removed from the solid carburizing agent and cooled using a multi-stage cooling method, with rapid cooling in the high temperature stage to inhibit the growth of austenite grains, slow cooling in the medium temperature stage to promote the uniform distribution and diffusion of carbon atoms, and rapid cooling in the low temperature stage to obtain the desired martensite or bainite structure.
[0026] Furthermore, the multi-stage cooling method is divided into three stages. The first stage uses water cooling to reduce the temperature of the steel to 500℃~550℃ for 20 minutes. The water cooling method uses high-pressure water to spray directly onto the surface of the steel. The high specific heat capacity and rapid heat conduction characteristics of water quickly remove the heat from the surface of the steel. During this process, the intensity and spray angle of the water flow need to be strictly controlled to ensure that the surface of the steel is cooled evenly and quickly while avoiding excessive thermal stress and deformation. The second stage uses air cooling to reduce the temperature of the steel to 200℃~250℃ for 1 hour. The air cooling method uses inert gas as the cooling medium. The cooling rate of the steel is controlled by adjusting the flow rate and temperature of the gas. During this process, the steel is placed in an air cooling chamber, and the gas flows over the surface of the steel to remove its heat. The third stage uses natural cooling to room temperature for 3 hours. The steel is placed in a room temperature environment and its temperature is reduced by natural convection and radiation heat transfer of the air. This process does not require additional cooling equipment or media. The steel only needs to be placed in a well-ventilated place.
[0027] It should be noted that, in this document, relational terms such as first and second, etc., are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Moreover, the terms "comprises," "comprising," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements but also other elements not explicitly listed, or elements inherent to such process, method, article, or apparatus.
[0028] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions, and variations may be made to these embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the appended claims and their equivalents.
Claims
1. A high-strength steel hot rolling preparation process, It is characterized in that The steps of hot rolling preparation of high-strength steel are as follows: S1. Prepare the following raw materials: 500-2000 parts of iron ore, 400-600 parts of coke, 300-500 parts of limestone, 125-500 parts of silicon, 100-500 parts of manganese, 50-300 parts of chromium, 50-200 parts of nickel, 10-100 parts of molybdenum, 10-50 parts of titanium, 5-50 parts of cerium, 10-100 parts of vanadium, 200-500 parts of desulfurizer, and 200-500 parts of dephosphorization agent; S2, putting the iron ore into a crusher for crushing; S3, putting iron ore, coke and limestone into the blast furnace until blast furnace gas and liquid iron are produced, and adding desulfurizer and dephosphorization agent; S4, adding blast furnace pig iron and silicon, silicon, manganese, chromium, nickel, molybdenum, titanium, cerium and vanadium into a steelmaking electric furnace for heating and smelting, and adding desulfurizer and desulfurizer again; S5, sending the refined molten steel into the LF refining furnace, and removing the inclusions and gas in the molten steel by RH vacuum degassing method; S6, the refined molten steel is continuously cast into a steel billet, and the continuously cast steel billet is sent to a heating furnace to eliminate internal stress; S7, sending the steel billet to the rough rolling mill for initial rolling to form a primary shape, and then sending the steel billet to the intermediate rolling mill for further rolling, and then finishing rolling under high temperature and high pressure; S8. After finishing rolling, the steel is rapidly cooled by water cooling and then quality tested.
2. The high-strength steel hot rolling preparation process according to claim 1, It is characterized in that The high-strength steel is specifically composed of the following ingredients: 1080 parts of iron ore, 350 parts of coke, 320 parts of limestone, 270 parts of silicon, 288 parts of manganese, 180 parts of chromium, 120 parts of nickel, 45 parts of molybdenum, 40 parts of titanium, 27 parts of cerium, 64 parts of vanadium, 210 parts of desulfurizer, and 230 parts of dephosphorization agent.
3. The high-strength steel hot rolling preparation process according to claim 1, Features: In step S3, the heating temperature of the blast furnace is 1200°C-1500°C, and the heating and melting time is 4 hours.
4. The high-strength steel hot rolling preparation process according to claim 1, Features: The timing of adding alloying elements in step S4 is: A1. Silicon is added at the beginning of the reduction period, and it takes 10 minutes to ensure that the ferrosilicon is completely melted; A2. Manganese is added after the slagging and carbon addition operations are completed; A3. Chromium is added at the beginning of the reduction period. After adding, the color of the slag needs to be observed. If it turns green, the reduction needs to be strengthened. A4. Nickel is added during the refining period; A5. Ferromolybdenum is added at the beginning of the reduction period; A6. Titanium is added in the late reduction period. Before adding, aluminum and titanium need to be added to the steel to deoxidize and stabilize nitrogen; A7. Cerium is added during the refining period; A8. Vanadium is added after the slag and molten steel are well deoxidized during the reduction period.
5. The high-strength steel hot rolling preparation process according to claim 1, It is characterized in that The operation method of the RH vacuum degassing method in step S5 is as follows: insert two immersion tubes at the bottom of the vacuum chamber into the molten steel, start the vacuum pump, evacuate the vacuum chamber, blow argon gas from about one-third of the lower part of the riser, and the gas in the molten steel is rapidly precipitated under the action of vacuum and is pumped away by the vacuum pump. The degassed molten steel is collected at the bottom of the vacuum chamber, and the undegassed molten steel enters the vacuum chamber from the riser and returns from the downcomer after degassing, forming a cycle. The number of cycles is 5, and the cycle time for each cycle is controlled at 3 minutes.
6. The high-strength steel hot rolling preparation process according to claim 1, Features: In step S6, the continuous casting speed is controlled at 3.0-7.0 m / min, the heating temperature is controlled at 1200° C.-1300° C., and the heating time is 3.5 h-6 h.
7. The high-strength steel hot rolling preparation process according to claim 1, Features: The quality inspection in step S8 includes appearance inspection, physical property test, metallographic structure inspection, non-destructive inspection and hardness inspection.
8. The high-strength steel hot rolling preparation process according to claim 1, Features: After the inspection is completed, the steel needs to be post-processed to improve its fatigue resistance.
9. The high-strength steel hot rolling preparation process according to claim 8, It is characterized in that The post-processing steps are: B1. Heat the steel to 850℃-1000℃ to make the solid carburizing agent fully contact with the steel surface; B2. Keep at 900℃ for 1 hour to allow carbon atoms to penetrate into the steel surface; B3. After carburizing is completed, the steel is taken out from the solid carburizing agent and cooled using a multi-stage cooling method.
10. The high-strength steel hot rolling preparation process according to claim 9, Features: The multi-stage cooling method is divided into three stages. The first stage uses water cooling to reduce the steel temperature to 500℃~550℃ for 20 minutes. The second stage uses air cooling to reduce the steel temperature to 200℃~250℃ for 1 hour. The third stage uses natural cooling to room temperature for 3 hours.
Citation Information
Cited By
Manufacturing method and application of low-temperature-resistant large-diameter seamless steel pipe
CN120479972A
A method for manufacturing large-diameter seamless steel pipe resistant to low temperatures and its application
CN120479972B