Preparation method of wear-resistant cutter
By pressurized composite of the ceramic body and the metal body and depositing an alumina layer on the surface, the problem of insufficient wear resistance of CNC machine tools is solved, and a high wear-resistant cutting head preparation is achieved.
Patent Information
- Application Number
- CN202410892333.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-15
AI Technical Summary
The wear resistance of existing CNC machine tools is insufficient and it is difficult to meet processing needs.
By pressing the ceramic body with a honeycomb structure and a metal body, and depositing an alumina layer on the surface of the composite molded body, an wear-resistant cutting cutter head is formed.
The wear resistance of the tool is significantly improved, combined with the antioxidant characteristics of the honeycomb structure and the alumina layer, the wear resistance of the tool is enhanced.
Abstract
Description
Technical Field
[0001] The invention relates to the field of numerical control machine tool processing, and in particular to a method for preparing a wear-resistant tool. Background Art
[0002] CNC machine tools are common processing equipment. CNC machine tools process workpieces. The common workpiece processing method is that a cutting tool cuts a certain type of incoming workpiece. However, how to obtain wear-resistant tools has always been the pursuit of the CNC machine tool industry.
[0003] Therefore, there is an urgent need to provide a method for preparing a wear-resistant tool. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a wear-resistant tool, wherein the prepared wear-resistant tool has the advantage of high wear resistance.
[0005] To achieve the above object, the present invention provides a method for preparing a wear-resistant tool, the method comprising the following steps:
[0006] S1: cleaning and drying the metal body and the ceramic body to obtain the pretreated metal body and the ceramic body, wherein the ceramic body has honeycomb holes and forms a honeycomb structure; S2: heating the metal body and the ceramic body, and pressurizing the preheated metal body and the ceramic body in a mold to form a composite molded body; S3: cooling the composite molded body to 300 degrees Celsius to 500 degrees Celsius, and then performing a tempering treatment; S4: depositing a deposition layer on the surface of the composite molded body, wherein the deposition layer is an aluminum oxide layer; S5: obtaining a wear-resistant cutting head.
[0007] Preferably, the pressure of the composite molding pressurization is 130 MPa to 150 MPa.
[0008] Preferably, the pore diameter of the honeycomb pores is 50 nanometers to 100 nanometers.
[0009] Preferably, step S4 further includes step S6, which is as follows: S6: testing the wear-resistant cutting head.
[0010] Preferably, step S6 is as follows: S61: the cutting head takes a sample and uses laser cladding technology to prepare a cladding coating material on the surface of the base material, and obtains a substrate sample and a coating sample; S62: multiple wear resistance tests are performed on the substrate sample and the coating sample, and the surface morphology before and after the wear resistance test is obtained using an electron microscope, and multiple substrate images and coating images are obtained respectively; S63: the substrate image and the coating image are compared to calculate the corrosion degree and obtain the wear resistance of the cutting head.
[0011] Preferably, the cleaning step in S1 is to ultrasonically clean the metal body and the ceramic body using anhydrous ethanol and ionized water.
[0012] Preferably, the cleaning time is 50 minutes to 70 minutes.
[0013] Compared with the prior art, the preparation method of the wear-resistant tool of the present invention pressurizes and composites a ceramic body with a honeycomb structure with a metal body, utilizes the characteristics of the honeycomb structure itself to greatly improve the wear resistance of the wear-resistant tool. In addition, a deposition layer is deposited on the surface of the composite molded body, and the anti-oxidation properties of aluminum oxide are utilized to improve the wear resistance of the tool. DETAILED DESCRIPTION
[0014] The technical solutions in the embodiments of the present application are clearly and completely described below in conjunction with specific implementation examples, and the technical solutions of the present invention are explained. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0015] Embodiment 1:
[0016] The preparation method of the wear-resistant tool of the present invention comprises the following steps:
[0017] S1: cleaning and drying the metal body and the ceramic body to obtain a pre-treated metal body and a ceramic body, wherein the ceramic body has honeycomb holes and forms a honeycomb structure;
[0018] S2: heating the metal body and the ceramic body, and pressurizing the preheated metal body and the ceramic body in a mold to form a composite molded body;
[0019] S3: Cooling the composite molded body to 300 degrees Celsius to 500 degrees Celsius and performing a tempering treatment;
[0020] S4: depositing a deposition layer on the surface of the composite molded body, wherein the deposition layer is an aluminum oxide layer;
[0021] S5: Obtain a wear-resistant cutting blade.
[0022] Compared with the prior art, the preparation method of the wear-resistant tool of the present invention pressurizes and composites a ceramic body with a honeycomb structure with a metal body, utilizes the characteristics of the honeycomb structure itself to greatly improve the wear resistance of the wear-resistant tool. In addition, a deposition layer is deposited on the surface of the composite molded body, and the anti-oxidation properties of aluminum oxide are utilized to improve the wear resistance of the tool.
[0023] Preferably, the pressure of the composite molding pressurization is 130 MPa to 150 MPa, and the composite molding effect is best at this pressure.
[0024] Preferably, the pore size of the honeycomb pores is 50 nanometers to 100 nanometers. When the pore size of the honeycomb pores is 50 nanometers to 100 nanometers, the stability of the overall structure is improved.
[0025] Preferably, the cleaning step in step S1 is to ultrasonically clean the metal body using anhydrous ethanol and ionized water. Ultrasonic cleaning with ionized water can improve uniformity, thereby improving the cleanliness of cleaning.
[0026] Preferably, the cleaning time is 50 to 70 minutes, and the optimal time is 60 minutes, at which time the cleanliness is the highest.
[0027] Embodiment 2:
[0028] The preparation method of the wear-resistant tool of the present invention comprises the following steps:
[0029] S1: cleaning and drying the metal body and the ceramic body to obtain a pre-treated metal body and a ceramic body, wherein the ceramic body has honeycomb holes and forms a honeycomb structure;
[0030] S2: heating the metal body and the ceramic body, and pressurizing the preheated metal body and the ceramic body in a mold to form a composite molded body;
[0031] S3: Cooling the composite molded body to 300 degrees Celsius to 500 degrees Celsius and performing a tempering treatment;
[0032] S4: depositing a deposition layer on the surface of the composite molded body, wherein the deposition layer is an aluminum oxide layer;
[0033] S5: Obtain a wear-resistant cutting blade.
[0034] S6: Testing the wear resistance of the cutting head.
[0035] The test steps are increased, and the wear resistance of the cutting blade head can be tested, thereby obtaining the wear resistance of the cutting blade head.
[0036] Embodiment three:
[0037] The preparation method of the wear-resistant tool of the present invention comprises the following steps:
[0038] S1: cleaning and drying the metal body and the ceramic body to obtain a pre-treated metal body and a ceramic body, wherein the ceramic body has honeycomb holes and forms a honeycomb structure;
[0039] S2: heating the metal body and the ceramic body, and pressurizing the preheated metal body and the ceramic body in a mold to form a composite molded body;
[0040] S3: Cooling the composite molded body to 300 degrees Celsius to 500 degrees Celsius and performing a tempering treatment;
[0041] S4: depositing a deposition layer on the surface of the composite molded body, wherein the deposition layer is an aluminum oxide layer;
[0042] S5: Obtain a wear-resistant cutting blade.
[0043] S6: cutting the cutter head to take samples and using laser cladding technology to prepare cladding coating materials on the surface of the base material, and obtaining base material samples and coating samples;
[0044] S7: performing multiple wear tests on the substrate sample and the coating sample, obtaining the surface morphology before and after the wear test using an electron microscope, and obtaining multiple substrate images and coating images respectively;
[0045] S8: Compare the substrate image and the coating image to calculate the corrosion degree and obtain the wear resistance of the cutting head.
[0046] The basic structure and working principle of the CNC machine tool involved in the present invention are well known to ordinary technicians in the field and will not be described in detail here.
[0047] It is obvious to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. At the same time, what is disclosed above is only the preferred embodiment of the present invention, and of course it cannot be used to limit the scope of the rights of the present invention. Therefore, equivalent changes made according to the scope of the patent application of the present invention are still within the scope covered by the present invention.
Claims
1. A method for preparing a wear-resistant tool, characterized in that: The preparation method of the wear-resistant tool comprises the following steps: S1: cleaning and drying the metal body and the ceramic body to obtain a pre-treated metal body and a ceramic body, wherein the ceramic body has honeycomb holes and forms a honeycomb structure; S2: heating the metal body and the ceramic body, and pressurizing the preheated metal body and the ceramic body in a mold to form a composite molded body; S3: cooling the composite molded body to 300 degrees Celsius to 500 degrees Celsius, and then performing a tempering treatment; S4: depositing a deposition layer on the surface of the composite molded body, wherein the deposition layer is an aluminum oxide layer; S5: Obtain a wear-resistant cutting blade.
2. The method for preparing a wear-resistant tool according to claim 1, characterized in that: The pressure of the composite molding pressurization is 130MPa to 150MPa.
3. The method for preparing a wear-resistant tool according to claim 1, characterized in that: The pore diameter of the honeycomb pores is 50 nanometers to 100 nanometers.
4. The method for preparing a wear-resistant tool according to claim 1, characterized in that: Step S4 also includes step S6, which is as follows: S6: Testing the wear-resistant cutting head.
5. The method for preparing a wear-resistant tool according to claim 4, characterized in that: Step S6 is as follows: S61: the cutting head takes samples and uses laser cladding technology to prepare a cladding coating material on the surface of the base material, and obtains a base material sample and a coating sample; S62: performing multiple wear tests on the substrate sample and the coating sample, obtaining the surface morphology before and after the wear test using an electron microscope, and obtaining multiple substrate images and coating images respectively; S63: Compare the substrate image and the coating image to calculate the corrosion degree and obtain the wear resistance of the cutting head.
6. The method for preparing a wear-resistant tool according to claim 1, characterized in that: The cleaning step in S1 is to ultrasonically clean the metal body and the ceramic body using anhydrous ethanol and ionized water.
7. The method for preparing a wear-resistant tool according to claim 6, characterized in that: The cleaning time is 50 to 70 minutes.