Piston ring with laser cladding coating
By using laser cladding technology to form the Ni-based alloy transition layer and Ni3Al/Cr7C3 cladding layer on the piston ring, the shortcomings in wear resistance and thermal load performance of the traditional piston ring are solved, and efficient and environmentally friendly coating preparation is achieved , meet the needs of high-end diesel engines.
Patent Information
- Application Number
- CN202310502862.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-06
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional piston rings have shortcomings in wear resistance, thermal load performance and environmental protection processes, and are difficult to meet the needs of high-end diesel engines and high-power gas engines.
The Ni-based alloy transition layer and Ni3Al/Cr7C3 cladding layer were formed on the outer circular surface of the piston ring. The Cr7C3 enhanced phase was diffusely distributed in the coating, and the combination of the laser cladding process was combined to improve the bonding performance of the coating and the substrate. Preparation efficiency.
The efficient combination of the coating and the substrate is achieved, which significantly improves the wear resistance and heat load resistance of the piston ring, while making the preparation process more environmentally friendly and efficient.
Smart Images

Figure CN118959594A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of piston rings, in particular to a laser cladding coating piston ring for an internal combustion engine. Background Art
[0002] Conventional piston rings generally use hard chrome, molybdenum spray coating or ceramic composite coating. The advantage of this type of piston ring is that the wear resistance is better than that of uncoated piston rings. The disadvantages include the following aspects:
[0003] Hard chrome and chrome ceramic composite coatings are generally prepared by electroplating methods with high pollution, which has low preparation efficiency and produces waste water, waste gas, waste residue and other wastes that pollute the environment. With the increasing requirements for green environmental protection, electroplating processes with high pollution will gradually be eliminated because they are not adapted to the needs of social development.
[0004] Sprayed molybdenum and molybdenum ceramic composite coatings are prepared by plasma spraying. The coatings are porous with a porosity of 10-25%, which can easily embed abrasive particles to form abrasive wear. The high porosity reduces the strength of the coatings, making them easy to break and peel off during use.
[0005] The above-mentioned electroplating coating and spray coating are mechanically bonded to the piston ring substrate, and are easily affected by the adverse effects of pre-treatment, and the bonding performance is not high.
[0006] The above factors will lead to the fact that the hard chrome, molybdenum spray coating and ceramic composite coating of traditional piston rings will be difficult to adapt to the needs of existing high-end diesel engines and high-strength coefficient diesel engines to be developed in the future. The market demand has higher wear resistance, thermal load performance, bonding performance and surface strengthening coating piston rings produced by green and environmentally friendly processes to meet the development needs of high-power, long-life, green and environmentally friendly new diesel engines and gas engines. Summary of the invention
[0007] The technical problem to be solved by the present invention is: in order to overcome the deficiencies in the prior art, a laser cladding coated piston ring is provided which has good coating-substrate bonding performance, higher wear resistance and heat load resistance, high coating preparation efficiency and is more environmentally friendly.
[0008] The technical solution adopted by the present invention is: a laser cladding coating piston ring, comprising a substrate, the outer cylindrical surface of the substrate is provided with a coating, and the coating comprises a Ni-based alloy transition layer and a Ni 3 Al / Cr 7 C 3 Cladding layer, Ni 3 Al / Cr 7 C 3 In-situ self-generated Cr is dispersed in the cladding layer. 7 C 3 Strengthening phase.
[0009] The Cr 7 C 3 The hardness of the strengthening phase is 2700HV, Cr 7 C 3 The wear resistance of the strengthening phase is good, so that the laser cladding piston ring has higher wear resistance;
[0010] Ni and Ni 3 Al-based materials are good heat-resistant materials, so the laser cladding piston ring has high heat-resistance load resistance.
[0011] Furthermore, the coating is formed on the outer cylindrical surface of the substrate by laser cladding, and the preparation process is more environmentally friendly and the preparation efficiency is greatly improved.
[0012] The laser cladding method specifically includes the following steps:
[0013] First, the outer cylindrical surface of the substrate is pretreated to remove attached oil stains and impurities;
[0014] Secondly, Ni-based alloy powder is clad on the outer cylindrical surface of the substrate by laser cladding to prepare a Ni-based alloy transition layer;
[0015] Then, Ni 3 Al / Cr 7 C 3 Alloy powder is clad on the surface of Ni-based alloy transition layer to prepare Ni 3 Al / Cr 7 C 3 Cladding layer;
[0016] Finally, the laser cladding coated piston ring is manufactured through machining.
[0017] Furthermore, the laser cladding method has the following parameters: the power of the laser cladding is 1200-1300 W, the scanning speed is 0.45-0.60 m / min, the laser beam is a circular spot, the diameter of the circular spot is 3 mm, and the powder feeding amount is 10-15 g / min.
[0018] Furthermore, the Cr 7 C 3 The strengthening phase is Ni 3 Al / Cr 7 C 3 The mass content of the cladding layer is 23-27%.
[0019] Furthermore, the coating has a thickness of 0.5 to 0.8 mm, the Ni-based alloy transition layer has a thickness of 0.2 to 0.3 mm, and the Ni 3 Al / Cr 7 C 3The thickness of the cladding layer is 0.3 to 0.5 mm.
[0020] Furthermore, the Ni 3 Al / Cr 7 C 3 The hardness of the cladding layer is 500-700 HV.
[0021] Furthermore, the material of the substrate includes but is not limited to ductile iron, vermicular cast iron, alloy cast iron and steel materials.
[0022] Compared with the prior art, the present invention has the following advantages: in the coating of the piston ring of the present invention, a Ni-based alloy is used as a transition layer. 3 Cr is dispersed in Al matrix 7 C 3 Laser cladding coating, Cr 7 C 3 The hardness of the strengthening phase is 2700HV, Cr 7 C 3 The wear resistance of the strengthening phase is good, so that the laser cladding piston ring has higher wear resistance; Ni and Ni 3 Al-based materials are good heat-resistant materials, which makes the laser cladding piston ring have high heat load resistance. The coating is formed on the outer cylindrical surface of the substrate by laser cladding, and the preparation process is more environmentally friendly and the preparation efficiency is greatly improved.
[0023] The laser cladding coated piston ring of the present invention has good bonding performance between the coating and the substrate, higher wear resistance and heat load resistance, high coating preparation efficiency and is more environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic diagram of the structure of the present invention;
[0025] Figure 2 It is a schematic diagram of the structure of the laser cladding coating of the present invention.
[0026] Numbers in the figure: 1-matrix, 2-Ni-based alloy transition layer, 3-Ni 3 Al / Cr 7 C 3 Cladding layer. DETAILED DESCRIPTION
[0027] The embodiments of the present invention are described in detail below. The embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following embodiments.
[0028] A laser cladding coating piston ring comprises a substrate 1, an outer cylindrical surface of the substrate 1 is provided with a coating, and the coating comprises a Ni-based alloy transition layer 2 and a Ni3 Al / Cr 7 C 3 Cladding layer 3, Ni 3 Al / Cr 7 C 3 Cr is dispersed in the cladding layer 3. 7 C 3 Strengthening phase.
[0029] The coating is formed on the outer circumferential surface of the substrate 1 by laser cladding, and the laser cladding method specifically includes the following steps:
[0030] First, the outer cylindrical surface of the substrate 1 is pre-treated to remove attached oil stains and impurities;
[0031] Secondly, Ni-based alloy powder is clad on the outer circumferential surface of the substrate 1 by laser cladding to prepare a Ni-based alloy transition layer 2;
[0032] Then, Ni 3 Al / Cr 7 C 3 Alloy powder is clad on the surface of Ni-based alloy transition layer 2 to prepare Ni 3 Al / Cr 7 C 3 Cladding layer 3;
[0033] Finally, the laser cladding coated piston ring is manufactured through machining.
[0034] The laser cladding method has the following parameters: the power of the laser cladding is 1200-1300W, the scanning speed is 0.45-0.60m / min, the laser beam is a circular spot, the diameter of the circular spot is 3mm, and the powder feeding amount is 10-15g / min.
[0035] Cr 7 C 3 The strengthening phase is Ni 3 Al / Cr 7 C 3 The mass content of the cladding layer 3 is 23-27%.
[0036] The thickness of the cladding coating is 0.5-0.8 mm, the thickness of the Ni-based alloy transition layer is 0.2-0.3 mm, and the Ni 3 Al / Cr 7 C 3 The thickness of the cladding layer 3 is 0.3 to 0.5 mm.
[0037] The hardness of the coating is 500-700 HV.
[0038] The material of the substrate 1 includes but is not limited to ductile iron, vermicular cast iron, alloy cast iron and steel materials.
Claims
1. A laser cladding coated piston ring, comprising a substrate (1), It is characterized in that The outer circumferential surface of the substrate (1) is provided with a coating, and the coating comprises, from the inside to the outside, a Ni-based alloy transition layer (2) and a Ni 3 Al / Cr 7 C 3 Cladding layer (3), Ni 3 Al / Cr 7 C 3 The in-situ self-generated Cr is dispersed in the cladding layer (3). 7 C 3 Strengthening phase.
2. The laser cladding coated piston ring according to claim 1, It is characterized in that The coating is prepared on the outer circumferential surface of the substrate (1) by laser cladding, which specifically includes the following steps: First, the outer circumferential surface of the substrate (1) is pre-treated to remove attached oil stains and impurities; Secondly, Ni-based alloy powder is clad on the outer circumferential surface of the substrate (1) by laser cladding to prepare a Ni-based alloy transition layer (2); Then, Ni 3 Al / Cr 7 C 3 The alloy powder is melt-coated on the surface of the Ni-based alloy transition layer (2) to prepare Ni 3 Al / Cr 7 C 3 Cladding layer (3); Finally, the laser cladding coated piston ring is manufactured through machining.
3. The laser cladding coated piston ring according to claim 2, It is characterized in that The laser cladding method has the following parameters: the power of the laser cladding is 1200-1300 W, the scanning speed is 0.45-0.60 m / min, the laser beam is a circular spot with a diameter of 3 mm, and the powder feeding amount is 10-15 g / min.
4. The laser cladding coated piston ring according to claim 1, It is characterized in that The Cr 7 C 3 The strengthening phase is Ni 3 Al / Cr 7 C 3 The mass content of the cladding layer (3) is 23-27%.
5. The laser cladding coated piston ring according to claim 1, It is characterized in that The coating has a thickness of 0.5 to 0.8 mm, the Ni-based alloy transition layer (2) has a thickness of 0.2 to 0.3 mm, and the Ni 3 Al / Cr 7 C 3 The thickness of the cladding layer (3) is 0.3 to 0.5 mm.
6. The laser cladding coated piston ring according to claim 1, It is characterized in that The Ni 3 Al / Cr 7 C 3 The hardness of the cladding layer (3) is 500-700 HV.
7. The laser cladding coated piston ring according to claim 1, It is characterized in that The material of the substrate (1) includes but is not limited to ductile iron, vermicular cast iron, alloy cast iron and steel material.