Electric arc fuse wire additive manufacturing method of 321 stainless steel structure gradient material

Through the combination of arc fuse additive manufacturing and ultrasonic impact technology, the problems of complex processes, high costs and low deposition efficiency in the preparation of functional gradient materials are solved, and efficient and low-cost manufacturing of large and complex structures are achieved, and the process flow is simplified. Reduced manufacturing costs.

CN118976969AActive Publication Date: 2024-11-19HARBIN INSTITUTE OF TECHNOLOGY SUZHOU RESEARCH INSTITUTE +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411077876.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The prior art has problems such as complex process, high cost, low deposition efficiency and easy contamination when preparing functional gradient materials, and is particularly difficult to meet the low-cost manufacturing needs of large and complex structures.

Method used

The arc fuse additive manufacturing method is adopted and combined with ultrasonic impact technology. By adjusting the welding voltage, current, wire feeding speed and ultrasonic impact parameters of the deposited layer, the degree of recrystallization of different deposited layers is controlled, achieving the purpose of transition of the structure gradient.

Benefits of technology

It realizes efficient and low-cost preparation of tissue functional gradient materials for large and complex structures, improves deposition efficiency, simplifies process flow, reduces manufacturing costs, and avoids dust pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976969A_ABST
    Figure CN118976969A_ABST
Patent Text Reader

Abstract

The invention discloses an electric arc fuse additive manufacturing method for a 321 stainless steel structure gradient material, relates to the field of additive manufacturing, and aims to solve the problems of complex process, high cost, low deposition efficiency, easiness in pollution and limitation of forming size in the conventional structure gradient material preparation process. According to the method, control over the recrystallization degree of different deposition positions is achieved by matching different ultrasonic peening and arc fuse additive manufacturing process parameters, then the purpose of gradient transition of the tissue structure is achieved, and the metal FGM with the tissue structure gradient is prepared in this way. According to the method, relative continuous gradient transition of the large-scale functional gradient material with the complex structure organization structure can be achieved, and the effects of improving the deposition efficiency, simplifying the technological process and reducing the manufacturing cost are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of additive manufacturing, and in particular relates to an arc fuse additive manufacturing method for a 321 stainless steel tissue gradient material. Background Art

[0002] Functional Graded Materials (FGM) are materials with a continuous gradient in composition or structure. By continuously changing the composition and structure of the material, the interface disappears, so that the performance of the material changes slowly with the composition and structure of the material. In functional gradient materials, the organizational gradient refers to the gradual change in the spatial microstructure of the material. Compared with traditional vapor deposition and electrochemical deposition methods, the additive manufacturing method for preparing FGM has more advantages, mainly reflected in the simple process, easy control of functional gradients and a wide range of applications.

[0003] In summary, the current methods for preparing FGM by additive manufacturing are mainly concentrated on laser powder laying and laser powder feeding additive manufacturing. For example, 316L stainless steel and Inconel 718 high-temperature alloy functional gradient materials with different composition change rates are prepared by laser coaxial powder feeding directed energy deposition (Li Pengfei et al. Research on the microstructure and properties of 316L / IN718 functional gradient materials with different composition change rates by laser additive manufacturing [J]. Journal of Mechanical Engineering. 2022, 58, 17: 226-239). Another example is the preparation of W-Cu functional gradient materials by laser selective melting (Yan Anru. Research on the forming process and characteristics of W-Cu composite materials by selective laser melting [D]. Beijing University of Technology). Although laser additive manufacturing can better realize the deposition of different functional gradient materials, laser powder laying additive manufacturing has problems such as low deposition efficiency and limited forming size, while laser powder feeding additive manufacturing has problems such as easy powder contamination and high forming cost. Both methods are difficult to meet the low-cost manufacturing requirements of large-scale complex structure functional gradient materials. Therefore, it is necessary to explore new process methods to more efficiently and conveniently prepare large-scale tissue functional gradient materials with complex structures to meet the special application needs in biomedicine, electricity, optics, magnetism and other fields.

[0004] At present, laser additive manufacturing for preparing functional gradient materials mainly involves mixing different types of powders in a certain proportion, melting the mixed powders of different components under the action of a laser heat source, and continuously changing the composition ratio of the metal powder as the deposition proceeds, so that the dissimilar materials form a metallurgical bond, and finally obtain functional gradient materials. Although this method is flexible in manufacturing and has high forming accuracy, it has problems such as high manufacturing cost, low deposition efficiency, and easy pollution. Summary of the invention

[0005] The purpose of the present invention is to address the problems of complex process, high cost, low deposition efficiency, easy contamination and limited forming size in the existing preparation process of tissue gradient materials, and propose an arc fuse additive manufacturing method for 321 stainless steel tissue gradient materials.

[0006] The present invention provides an arc fuse additive manufacturing method for 321 stainless steel structure gradient material, which is carried out according to the following steps:

[0007] Step 1: After surface pretreatment of the metal substrate, fix and clamp it;

[0008] Step 2: Fix the welding gun and the robot arm together, and adjust the angle between the welding gun and the substrate surface;

[0009] Step 3: Setting the arc fuse additive manufacturing process, and performing arc fuse additive manufacturing to complete the formation of a deposition layer;

[0010] The arc fuse additive manufacturing process conditions are as follows: the diameter of the welding wire is 0.8 mm to 1.6 mm, the thickness of the substrate is greater than 5 mm, the welding voltage is 14 V to 22 V, the current is 126 A to 198 A, the wire feeding speed is 3.0 m / min to 8.0 m / min, the running speed is 0.1 m / min to 0.4 m / min, the welding wire elongation is 12 to 15 mm, the interlayer waiting time is 1 min, and the shielding gas is Ar+CO with a flow rate of 15 L / min to 20 L / min 2 ;

[0011] Step 4: After completing the formation of one deposited layer, perform ultrasonic impact treatment; after the ultrasonic impact, adjust the wire feeding speed, welding voltage and welding current in the arc fuse additive manufacturing process in step 3, and continue to deposit on the basis of completing one deposited layer until the deposition is completed; wherein, adjusting the arc fuse additive manufacturing process in step 3 means that the values ​​of the wire feeding speed, welding voltage and welding current increase gradually with the increase of the deposited layer.

[0012] Furthermore, in step 2, the angle between the welding gun and the substrate surface is adjusted to 10° to 15°.

[0013] Furthermore, the arc fuse additive manufacturing process parameters described in step 3 are as follows: the diameter of the welding wire is 1.0 mm to 1.4 mm, the thickness of the substrate is greater than 5 mm, the welding voltage is 16 V to 20 V, the current is 140 A to 180 A, the wire feeding speed is 5.0 m / min to 7.0 m / min, the running speed is 0.2 m / min to 0.3 m / min, the welding wire elongation is 13 to 15 mm, the interlayer waiting time is 1 min, and the shielding gas is Ar+CO with a flow rate of 15 L / min to 20 L / min. 2 .

[0014] Furthermore, the arc fuse additive manufacturing process parameters described in step 3 are as follows: the diameter of the welding wire is 1.0 mm to 1.2 mm, the thickness of the substrate is greater than 5 mm, the welding voltage is 15 V to 18 V, the current is 130 A to 160 A, the wire feeding speed is 4.0 m / min to 6.0 m / min, the running speed is 0.2 m / min to 0.3 m / min, the welding wire elongation is 13 to 15 mm, the interlayer waiting time is 1 min, and the shielding gas is Ar+CO with a flow rate of 15 L / min to 20 L / min. 2 .

[0015] Furthermore, the gradient increase with the increase of deposition layers described in step 4 means that for every 4 deposition layers, the arc fuse additive manufacturing process in step 3 means that the values ​​of wire feeding speed, welding voltage and welding current increase by a gradient.

[0016] Further, after adjusting the wire feeding speed, welding voltage and welding current in the arc fuse additive manufacturing process in step 3 in step 4, the deposition is continued on the basis of completing one deposition layer until the deposition is completed, which is carried out in the following manner:

[0017] When the deposition layer is 1 to 4 layers, the arc fuse additive manufacturing process parameters are as follows: the wire diameter is 0.8 mm to 1.6 mm, the substrate thickness is greater than 5 mm, the welding voltage is 14 V to 15 V, the current is 126 A to 139 A, the wire feeding speed is 4.0 m / min to 5.0 m / min, the running speed is 0.1 m / min to 0.4 m / min, the wire elongation is 12 to 15 mm, the interlayer waiting time is 1 min, and the shielding gas is Ar+CO with a flow rate of 15 L / min to 20 L / min. 2 ;

[0018] When the deposition layer is 5 to 8 layers, the arc fuse additive manufacturing process parameters are as follows: the wire diameter is 0.8 mm to 1.6 mm, the substrate thickness is greater than 5 mm, the welding voltage is 15 V to 15.5 V, the current is 139 A to 165 A, the wire feeding speed is 5.0 m / min to 6.0 m / min, the running speed is 0.1 m / min to 0.4 m / min, the wire elongation is 12 to 15 mm, the interlayer waiting time is 1 min, and the shielding gas is Ar+CO with a flow rate of 15 L / min to 20 L / min. 2 ;

[0019] When the deposition layer is 9 to 12 layers, the arc fuse additive manufacturing process parameters are as follows: the wire diameter is 0.8 mm to 1.6 mm, the substrate thickness is greater than 5 mm, the welding voltage is 15.5 V to 16 V, the current is 165 A to 195 A, the wire feeding speed is 6.0 m / min to 8.0 m / min, the running speed is 0.1 m / min to 0.4 m / min, the wire elongation is 12 to 15 mm, the interlayer waiting time is 1 min, and the shielding gas is Ar+CO with a flow rate of 15 L / min to 20 L / min. 2 ;

[0020] When the deposition layer is more than 12 layers, the arc fuse additive manufacturing process parameters are as follows: the wire diameter is 0.8mm~1.6mm, the substrate thickness is greater than 5mm, the welding voltage is 16V~22V, the current is 165A~198A, the wire feeding speed is 6.0m / min~8.0m / min, the running speed is 0.1m / min~0.4m / min, the wire elongation is 12~15mm, the interlayer waiting time is 1min, and the shielding gas is Ar+CO with a flow rate of 15L / min~20L / min 2 .

[0021] Furthermore, in step 4, the ultrasonic impact device of the ultrasonic impact treatment is perpendicular to the substrate and has an angle of 90° with the deposited layer.

[0022] Furthermore, the ultrasonic impact parameters of the ultrasonic impact treatment in step 4 are: impact power 600W to 1200W, impact frequency 18 to 25kHz, impact running speed 0.05m / min to 0.2m / min, and applied load 40N to 100N.

[0023] Furthermore, the ultrasonic impact parameters of the ultrasonic impact treatment in step 4 are: impact power 800W-1000W, impact frequency 20-25kHz, impact running speed 0.1m / min-0.2m / min, and applied load 60N-100N.

[0024] Furthermore, the ultrasonic impact parameters of the ultrasonic impact treatment in step 4 are: impact power 600W-800W, impact frequency 18-22kHz, impact running speed 0.05m / min-0.1m / min, and applied load 40N-80N.

[0025] The main technical solution of the present invention is: introducing ultrasonic impact means in the arc fuse additive manufacturing process, using different deposition parameters and ultrasonic impact parameters to match to obtain an adjustable degree of recrystallization, and then realizing tissue gradient transition at different deposition stages, ultimately achieving the purpose of preparing tissue gradient transition.

[0026] The theoretical basis of this technical solution is as follows:

[0027] After the ultrasonic impact is introduced in the arc fuse additive manufacturing process, it can have two important effects on the deposited layer: first, under the action of ultrasonic impact, the surface of the deposited layer will form severe plastic deformation, forming a large number of dislocation increments, resulting in obvious lattice distortion, and then introducing a large amount of deformation energy storage in the structure. The size of the deformation energy storage directly affects the strength of the driving force of the recrystallization degree. Specifically, as shown in formula (1), the grain boundary driving force ΔE can be expressed as:

[0028]

[0029] τ is the energy per unit length of the dislocation line, ρ NR is the dislocation density before recrystallization, ρ(x) is the dislocation density after grain boundary migration, and r is the grain radius. These changes will undergo recrystallization under the influence of the subsequent arc fuse additive manufacturing thermal effect, achieving a certain degree of grain refinement. However, under the combined effect of different deformation energy storage and arc fuse additive manufacturing interlayer thermal effect, the difference in recrystallization activation energy will lead to significantly different degrees of recrystallization in the deposited layer. The ZenerHollomon parameter Z can be expressed as:

[0030]

[0031] is the strain rate, T is the deformation temperature, Q is the recrystallization activation energy, and R is the gas constant. Second, in addition to surface plastic deformation, ultrasonic impact can also produce ultrasonic oscillation under the action of high strain in a very short time. Ultrasonic oscillation will break some dislocation constraints and promote the movement of dislocations. Dislocations will undergo a large number of mergers and annihilations during the movement process, forming a large number of substructures, and the substructure ratio f LAGB The relationship with the recrystallization percentage A is as follows:

[0032] f LAGB ∝A(3)

[0033] This means that the change in the proportion of substructures caused by ultrasonic impact will directly affect the percentage of recrystallization. Based on the above changes in the deposited layer caused by ultrasonic impact, it can be seen that a certain degree of recrystallization will occur under the combined action of ultrasonic impact and the interlayer thermal effect of arc fuse additive manufacturing, and the occurrence of recrystallization will cause grain refinement. The specific schematic diagram is shown in the figure.

[0034] Based on this principle, the present invention proposes to control the degree of recrystallization at different deposition positions by matching different ultrasonic impact and arc fuse additive manufacturing process parameters, thereby achieving the purpose of structural gradient transition, and in this way preparing metal FGM with structural gradient.

[0035] The present invention focuses on the additive manufacturing of nuclear metal structure gradient materials. In view of the problems of complex process, high cost and limited forming size in the preparation of structure functional gradient materials at the current stage, it is proposed to realize the difference in recrystallization degree of different deposited layers by combining ultrasonic impact with arc fuse additive manufacturing technology to achieve the purpose of structure gradient transition. Combined with the physical properties and recrystallization conditions of the deposited metal, the ultrasonic impact process (introducing deformation and substructure) and the forming process (introducing interlayer thermal effect) are scientifically matched according to the different designed structure transition conditions, and the arc fuse method is used to realize high deposition efficiency, high quality and high performance arc fuse additive manufacturing of structure functional gradient materials.

[0036] The present invention has the following beneficial effects:

[0037] The present invention adopts ultrasonic impact combined with arc fuse additive manufacturing to realize the preparation of structural functional gradient materials. The key technical points that can be achieved by the invention are: reasonably setting the structural gradient transition mode (including the structural composition of each deposited layer and the transition efficiency) according to the characteristics of the deposited metal, scientifically matching the ultrasonic impact process under different structures (including impact power, impact frequency, impact running speed, external load and number of processing times) and the arc fuse additive manufacturing forming process (including welding voltage, welding current, wire feeding speed, running speed, interlayer waiting time and elongation, etc.) and formulating process control points specifically suitable for the preparation of structural functional gradient materials.

[0038] Compared with laser additive manufacturing to prepare functional gradient materials of organizational structure, the present invention has the advantages of high forming efficiency, low cost, no limitation on the size of formed parts, and no dust pollution.

[0039] Compared with traditional vapor deposition and electrochemical deposition methods, this technology has the advantages of simple process flow and high stability when forming complex structural parts.

[0040] Compared with conventional ultrasonic impact treatment assisted arc fuse additive manufacturing, the present invention can not only achieve the purposes of grain refinement, improvement of stress state, defect repair and reduction of anisotropy, but also realize the control of organizational structure gradient by reasonably matching with the interlayer thermal effect of arc fuse additive manufacturing.

[0041] The present invention can realize relatively continuous gradient transition of large-scale complex structural organizational structure functional gradient materials, thereby achieving the effects of improving deposition efficiency, simplifying process flow and reducing manufacturing costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 Schematic diagram of the tissue gradient transition principle;

[0043] Figure 2 Schematic diagram of ultrasonic impact treatment of the workpiece after deposition;

[0044] Figure 3 Comparison diagram of the structure gradient material formed by the present invention and conventional arc fuse additive manufacturing; wherein, (ac) the structure of the deposited layer not treated by the present invention, (df) the structure of the deposited layer treated by the present invention;

[0045] Figure 4 Comparison diagram of the structure formed by the present invention and conventional arc fuse additive manufacturing; wherein, (a) conventional arc fuse additive manufacturing structure, (b) the structure of the deposited layer after processing by the present invention;

[0046] Figure 5 The morphology of the recrystallized grains inside the formed part of the present invention;

[0047] Figure 6 Comparison of the degree of recrystallization of the product of the present invention and conventional arc fuse additive manufacturing: (a) conventional arc fuse additive manufacturing recrystallization distribution, (b) the recrystallization distribution of the deposited layer after treatment by the present invention;

[0048] Figure 7 Schematic diagram of the process flow of the present invention. DETAILED DESCRIPTION

[0049] In order to make the objectives, technical solutions and advantages of the embodiments of the present invention more clearly understood, the spirit of the contents disclosed by the present invention will be described in detail below. After understanding the embodiments of the contents of the present invention, any technician in the relevant technical field can change and modify them according to the techniques taught by the contents of the present invention without departing from the spirit and scope of the contents of the present invention.

[0050] The exemplary embodiments of the present invention and the description thereof are used to explain the present invention but are not intended to limit the present invention.

[0051] Embodiment 1:

[0052] The present invention uses ultrasonic impact and arc fuse additive manufacturing to prepare 321 stainless steel structure gradient materials, achieving high efficiency and low cost manufacturing of metal-based structure gradient materials. The specific implementation steps are as follows:

[0053] (1) Organizational structure gradient transition design

[0054] In order to effectively achieve the transition of the structural function gradient between different deposited layers, the structural design based on the characteristics of the deposited metal and the recrystallization conditions is one of the important factors affecting the transition effect. The present invention scientifically matches the ultrasonic impact process parameters and the arc fuse additive manufacturing process parameters according to formulas (1) to (3). In the actual forming process, the ultrasonic impact process parameters are set as shown in Table 1.

[0055] Table 1 Ultrasonic impact process parameter settings

[0056]

[0057] To match this, the process parameter settings of the arc fuse additive manufacturing are shown in Table 2.

[0058] Table 2 Arc fuse additive manufacturing process settings

[0059]

[0060] (2) Forming method

[0061] After completing the process matching of ultrasonic impact and arc fuse additive manufacturing, 304 stainless steel was used as the substrate (thickness 5 mm) and 321 stainless steel wire (diameter 1.2 mm) was used as the deposited metal. The chemical compositions of the substrate and wire are shown in Table 3.

[0062] Table 3 Chemical composition of substrate and wire (mass percentage)

[0063]

[0064] During the deposition process, alcohol is used to clean the surface of the substrate to remove oil and oxide layer, the substrate is clamped and fixed, the welding gun, ultrasonic impact equipment and robotic arm are connected, and the forming and ultrasonic impact treatment of the deposited metal are completed through path planning software and control units. First, the deposition of 321 stainless steel material is realized. After a certain interlayer waiting time, the deposited layer is cooled to below 100°C (this is mainly because too high a temperature of the deposited layer will cause damage to the ultrasonic impact equipment). At this time, after a certain cleaning treatment of the deposited layer, the external load and running trajectory of the ultrasonic impact equipment are controlled by the robotic arm. After the impact is completed, the deposition continues on the previously treated deposited layer. Under the combined action of ultrasonic impact and arc fuse interlayer thermal effect, a certain recrystallization will occur, achieving a certain grain refinement effect. After obtaining 1-4 deposited layers under this process, the parameter matching of ultrasonic impact and arc fuse additive manufacturing is adjusted, and the previous process is repeated to achieve a higher degree of recrystallization and make the organization more refined. The obtained 5-8 deposited layers form a clear organizational structure gradient compared with the initial 1-4 deposited layers. After adjusting the specific parameters according to this mode, continue to deposit 9-12 layers of deposition, and finally achieve the gradient transition of the organizational structure. The specific effect is shown in Figure 3 .

[0065] (3) Microstructure refinement and recrystallization

[0066] Compared with the 321 stainless steel structure gradient metal product (hereinafter referred to as the traditional product) manufactured by the ultrasonic impact process arc fuse additive manufacturing method omitted in Example 1, the structure obtained by the present invention is significantly refined, and the structure undergoes an obvious transformation from columnar crystal to equiaxed crystal under the action of recrystallization. The specific situation is as follows Figure 4 As shown in Figure 2, after recrystallization occurs, a large number of typical recrystallized grains will be formed in the structure. Figure 5 As shown (BF is bright field image, DF is dark field image), the recrystallization comparison is as follows Figure 6 shown.

[0067] (4) Tensile properties

[0068] The tensile properties of the parts formed by the present invention are significantly improved in the X, Y and Z directions compared with the parts made by conventional arc fuse additive manufacturing, as shown in Table 4.

[0069] Table 4 Comparison of tensile properties between conventional arc fuse additive manufacturing parts and the parts of the present invention

[0070]

[0071] (5) Impact performance

[0072] The impact performance of the parts formed by the present invention (sample size is 10mm×10mm×55mm, room temperature) is significantly improved in the X, Y and Z directions compared with the parts made by conventional arc fuse additive manufacturing, as shown in Table 5.

[0073] Table 5 Comparison of impact performance between conventional arc fuse additive manufacturing parts and the parts of the present invention

[0074]

[0075]

Claims

1. An arc fuse additive manufacturing method for 321 stainless steel structure gradient material, characterized in that It is carried out according to the following steps: Step 1: After surface pretreatment of the metal substrate, fix and clamp it; Step 2: Fix the welding gun and the robot arm together, and adjust the angle between the welding gun and the substrate surface; Step 3: Setting the arc fuse additive manufacturing process, and performing arc fuse additive manufacturing to complete the formation of a deposition layer; The arc fuse additive manufacturing process conditions are as follows: the diameter of the welding wire is 0.8 mm to 1.6 mm, the thickness of the substrate is greater than 5 mm, the welding voltage is 14 V to 22 V, the current is 126 A to 198 A, the wire feeding speed is 3.0 m / min to 8.0 m / min, the running speed is 0.1 m / min to 0.4 m / min, the welding wire elongation is 12 to 15 mm, the interlayer waiting time is 1 min, and the shielding gas is Ar+CO2 with a flow rate of 15 L / min to 20 L / min; Step 4: After completing the formation of one deposited layer, perform ultrasonic impact treatment; after the ultrasonic impact, adjust the wire feeding speed, welding voltage and welding current in the arc fuse additive manufacturing process in step 3, and continue to deposit on the basis of completing one deposited layer until the deposition is completed; wherein, adjusting the arc fuse additive manufacturing process in step 3 means that the values ​​of the wire feeding speed, welding voltage and welding current increase gradually with the increase of the deposited layer.

2. The arc fuse additive manufacturing method of 321 stainless steel structure gradient material according to claim 1 is characterized in that In step 2, the angle between the welding gun and the substrate surface is adjusted to 10° to 15°.

3. The arc fuse additive manufacturing method of 321 stainless steel structure gradient material according to claim 1 is characterized in that The arc fuse additive manufacturing process parameters described in step 3 are as follows: a wire diameter of 0.8 mm to 1.6 mm, a substrate thickness greater than 5 mm, a welding voltage of 16 V to 20 V, a current of 140 A to 180 A, a wire feeding speed of 5.0 m / min to 7.0 m / min, a running speed of 0.2 m / min to 0.3 m / min, a wire elongation of 13 to 15 mm, an interlayer waiting time of 1 min, and a shielding gas of Ar+CO2 with a flow rate of 15 L / min to 20 L / min.

4. The arc fuse additive manufacturing method of 321 stainless steel structure gradient material according to claim 1 is characterized in that The arc fuse additive manufacturing process parameters described in step 3 are as follows: a wire diameter of 0.8 mm to 1.6 mm, a substrate thickness greater than 5 mm, a welding voltage of 15 V to 18 V, a current of 130 A to 160 A, a wire feeding speed of 4.0 m / min to 6.0 m / min, a running speed of 0.2 m / min to 0.3 m / min, a wire elongation of 13 to 15 mm, an interlayer waiting time of 1 min, and a shielding gas of Ar+CO2 with a flow rate of 15 L / min to 20 L / min.

5. The arc fuse additive manufacturing method of 321 stainless steel structure gradient material according to claim 1, characterized in that The gradient increase with the increase of deposition layers described in step 4 means that for every 4 deposition layers, the arc fuse additive manufacturing process in step 3 means that the values ​​of wire feeding speed, welding voltage and welding current increase by one gradient.

6. The arc fuse additive manufacturing method of 321 stainless steel tissue gradient material according to claim 1 or 5, characterized in that After adjusting the wire feed speed, welding voltage and welding current in the arc fuse additive manufacturing process in step 3 as described in step 4, continuing to deposit on the basis of completing one deposition layer until the deposition is completed is performed in the following manner: When the deposition layer is 1 to 4 layers, the arc fuse additive manufacturing process parameters are as follows: the wire diameter is 0.8 mm to 1.6 mm, the substrate thickness is greater than 5 mm, the welding voltage is 14 V to 15 V, the current is 126 A to 139 A, the wire feeding speed is 4.0 m / min to 5.0 m / min, the running speed is 0.1 m / min to 0.4 m / min, the wire elongation is 12 to 15 mm, the interlayer waiting time is 1 min, and the shielding gas is Ar+CO2 with a flow rate of 15 L / min to 20 L / min; When the deposition layer is 5 to 8 layers, the arc fuse additive manufacturing process parameters are: wire diameter 0.8 mm to 1.6 mm, substrate thickness greater than 5 mm, welding voltage 15 V to 15.5 V, current 139 A to 165 A, wire feeding speed 5.0 m / min to 6.0 m / min, running speed 0.1 m / min to 0.4 m / min, wire elongation 12 to 15 mm, interlayer waiting time 1 min, shielding gas flow rate 15 L / min to 20 L / min Ar + CO2; When the deposition layer is 9 to 12 layers, the arc fuse additive manufacturing process parameters are: wire diameter of 0.8 mm to 1.6 mm, substrate thickness greater than 5 mm, welding voltage of 15.5 V to 16 V, current of 165 A to 195 A, wire feeding speed of 6.0 m / min to 8.0 m / min, running speed of 0.1 m / min to 0.4 m / min, wire elongation of 12 to 15 mm, interlayer waiting time of 1 min, and shielding gas of Ar+CO2 with a flow rate of 15 L / min to 20 L / min; When the deposition layer is more than 12 layers, the arc fuse additive manufacturing process parameters are as follows: wire diameter of 0.8mm~1.6mm, substrate thickness greater than 5mm, welding voltage of 16V~22V, current of 165A~198A, wire feeding speed of 6.0m / min~8.0m / min, running speed of 0.1m / min~0.4m / min, wire elongation of 12~15mm, interlayer waiting time of 1min, and shielding gas of Ar+CO2 with a flow rate of 15L / min~20L / min.

7. The arc fuse additive manufacturing method of 321 stainless steel structure gradient material according to claim 1, characterized in that In step 4, the ultrasonic impact device for ultrasonic impact treatment is perpendicular to the substrate and has an angle of 90° with the deposited layer.

8. The arc fuse additive manufacturing method of 321 stainless steel structure gradient material according to claim 1 or 7, characterized in that The ultrasonic impact parameters of the ultrasonic impact treatment in step 4 are: impact power 600W to 1200W, impact frequency 18 to 25kHz, impact running speed 0.05m / min to 0.2m / min, and applied load 40N to 100N.

9. The arc fuse additive manufacturing method of 321 stainless steel structure gradient material according to claim 8, characterized in that The ultrasonic impact parameters of the ultrasonic impact treatment in step 4 are: impact power 800W-1200W, impact frequency 20-25kHz, impact running speed 0.05m / min-0.15m / min, and applied load 60N-100N.

10. The arc fuse additive manufacturing method of 321 stainless steel structure gradient material according to claim 1, characterized in that The ultrasonic impact parameters of the ultrasonic impact treatment in step 4 are: impact power 1000W~1200W, impact frequency 22~25kHz, impact running speed 0.05m / min~0.1m / min, and external load 80N~100N.

Citation Information

Patent Citations

  • Laser additive manufacturing method for homogeneous functionally graded material and structure

    CN104190930A

  • Method for preparing metal gradient material through selective laser melting

    CN111992717A

  • Method for gradient regulation and control of technological parameter in additive manufacturing process

    WO2021004185A1