Method for preparing polyphenyl ether particles
By controlling the precipitation size and drying conditions of polyphenylene ether particles, using a rotary cylindrical dryer and high-temperature nitrogen, the problem of coking during the polyphenylene ether drying process is solved, and the production and reduction equipment of high-quality polyphenylene ether powder are realized. Risk of blockage.
Patent Information
- Application Number
- CN202411157012.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-22
AI Technical Summary
Coking and adhesion are prone to occur during the drying process of polyphenylene ether, resulting in equipment scaling and product quality decline. The existing technology solutions are complex, costly and unsatisfactory.
By controlling the precipitation size of polyphenylene ether particles, the solvent composition during filtration and washing, as well as the temperature and heat source during the drying process, the rotary cylindrical dryer and high-temperature nitrogen are used to dry to ensure the average particle size of polyphenylene ether particles. More than 120 microns, moisture content is less than 50%, and coking is avoided by optimizing the composition of the wash and dryer design.
It effectively avoids coking during drying, improves the quality and production efficiency of polyphenylene ether powder, reduces the degree of flying and the risk of pipeline blockage, and improves the yield.
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing polyphenylene ether particles. Background Art
[0002] Polyphenylene ether is a general engineering plastic with excellent dielectric properties, temperature resistance, and water resistance. Its products have high tensile strength and impact strength, and are self-extinguishing.
[0003] Polyphenylene ether is usually obtained by using xylenol as a raw material, and reacting with oxygen in an organic solvent with metal salts and amines as catalysts to undergo an oxidative coupling reaction. The reaction mixture is then precipitated, filtered, washed, and dried to obtain polyphenylene ether powder, as described in patents US20170275434, CN107236124A, CN104136490B, CN103154086B, and CN103421181A.
[0004] In fact, in the drying process of large-scale production, due to the presence of solvents in polyphenylene ether particles, polyphenylene ether particles are prone to melt, coke and stick together when heated to remove the solvent, resulting in scaling in the dryer and coking in the product, seriously affecting product quality. Patent CN111978535B discloses a method for manufacturing polyphenylene ether to reduce scaling of the dryer during drying, which requires the installation of a series of dryers, and the equipment and operation are complex, the cost is high, and the actual effect is not ideal.
[0005] Therefore, a method for producing polyphenylene ether particles is needed to further reduce the possibility of coking during the drying process of the polyphenylene ether particles. Summary of the invention
[0006] Problems to be solved by the invention As described above, the risk of coking and blocking occurring when drying polyphenylene ether using the techniques disclosed so far is still high.
[0007] Therefore, the object of the present invention is to provide a method for reducing the coking problem during the drying process of polyphenylene ether particles.
[0008] Means of solving problems The inventors conducted in-depth research on the above-mentioned problem and found that by controlling the particle size during the precipitation of polyphenylene ether, controlling the solvent composition during filtration and washing, controlling the drying temperature during drying, and using nitrogen as a heat source, coking during the drying process can be effectively avoided.
[0009] The present invention is as follows: [1] During the polymerization and precipitation process, the ratio of good solvent to poor solvent is used to control the size of the precipitated polyphenylene ether particles to be suitable, with an average particle size greater than 120 μm; [2] Filtration and washing process, when the polyphenylene ether particles are filtered and washed, they are washed with a water-containing washing liquid, the washing liquid is composed of an alcohol compound and a washing accelerator, the washing accelerator contains water and dimethylamine, wherein the alcohol compound is 88-94.4%, the water content is 5-10%, and the dimethylamine content is 0.1-2%, and the moisture content of the polyphenylene ether particles after filtering and washing is controlled to be less than 50%; [3] The drying process is carried out using a rotary drum dryer, and high-temperature nitrogen is used as a heat source. The high-temperature nitrogen is introduced from the material discharge end of the rotary drum dryer and is discharged from the material feeding end carrying organic vapor. During the rotation of the dryer drum, the polyphenylene ether particles are continuously introduced from one end of the dryer and the dried polyphenylene ether particles are continuously discharged from the other end. [4] The weight average molecular weight of the polyphenylene ether is greater than 15,000.
[0010] Effects of the Invention 1. The method for preparing polyphenylene ether particles provided by the present invention can effectively avoid the occurrence of coking during the drying process and obtain high-quality polyphenylene ether powder.
[0011] 2. The preparation method of the polyphenylene ether particles provided by the present invention has an average particle size of 120 microns, which can effectively reduce the flying degree of the polyphenylene ether powder in the dryer, avoid pipeline blockage, and improve the yield. DETAILED DESCRIPTION
[0012] The following is a detailed description of a method for implementing the present invention (hereinafter referred to as "this embodiment"). The following this embodiment is an example for explaining the present invention, and the present invention is not limited to this embodiment, and the present invention can be implemented with appropriate modifications within the scope of the gist.
[0013] [Polyphenylene ether polymerization] The polyphenylene ether of this embodiment has a weight average molecular weight greater than 15,000 (determined by sol-gel chromatography), and is obtained by polymerizing xylenol monomer in an organic solvent, using a copper salt-amine as a catalyst, and xylenol and oxygen undergo an oxidative coupling reaction, and after the reaction, an organic acid is used as a terminator to treat the reaction solution.
[0014] An organic solvent, a phenolic monomer, a copper salt and an amine are added to a stirring reactor in a certain proportion. After adjusting to a set temperature, oxygen is introduced from the bottom of the reactor under stirring, and polymerization occurs. The temperature of the materials in the reactor is maintained within a certain range. After reaching the end point of the reaction, the oxygen is stopped to terminate the reaction, and a certain amount of organic acid is added to terminate the polymerization to obtain a mixed solution containing polyphenylene ether.
[0015] The xylenol refers to one or more of 2,6-dimethylphenol, 2,6-diethylphenol and 2,5-dimethylphenol.
[0016] The organic solvent refers to a good solvent for polyphenylene ether, including small molecular compounds containing a benzene ring, such as benzene, toluene, chlorobenzene, xylene, trimethylbenzene, etc., preferably toluene, chlorobenzene, and xylene.
[0017] The copper salt in this embodiment refers to a mixture of one or more of cupric chloride, cuprous chloride, cupric bromide, copper nitrate, copper sulfate, and the like.
[0018] Amine refers to an organic compound containing nitrogen and carbon elements, such as triethylamine, trimethylamine, tributylamine, aniline, cyclohexylamine, ethylenediamine, morpholine, p-phenylenediamine, dibutylamine, diethylamine, etc., or a mixture of several of them.
[0019] The oxygen in this embodiment has a purity greater than 95%, preferably a purity greater than 97%.
[0020] The organic acid used to terminate the reaction refers to a compound containing a carboxyl group, such as acetic acid, benzoic acid, EDTA, sodium salt of EDTA, etc.
[0021] [Precipitation and precipitation] The polyphenylene ether reaction liquid of this embodiment is contacted and mixed with a poor solvent to produce a precipitation process, and the size of the precipitated particles is controlled by the amount of the poor solvent added, and the mass content of the poor solvent is preferably 40-50%, and the average diameter of the obtained particles is greater than 120 microns. Wherein, the good solvent is an aromatic solvent such as xylene, chlorobenzene, toluene, etc.; the poor solvent is an alcohol solvent such as methanol, propylene glycol, ethanol, butanol, etc.
[0022] [Filtration and washing] In the filtering and washing process of the polyphenylene ether particles of this embodiment, the polyphenylene ether particles are first filtered by a filter to achieve liquid-solid separation. To further remove the impurities remaining in the particles, the polyphenylene ether filter cake is washed with a washing liquid. The washing liquid composition comprises an alcohol compound and a washing accelerator, wherein the alcohol compound is such as methanol, ethanol, propanol, butanol, etc., preferably methanol, and the washing accelerator comprises water and dimethylamine, wherein dimethylamine refers to a dimethylamine compound having a structure such as (CH3)2NX, wherein X is C 1-10 Alkyl substituents. The composition of the washing liquid: 88-94.4% alcohol compounds, 5-10% water content, 0.1-2% dimethylamine content. The moisture content of the filter cake after filtration is less than 50%.
[0023] [dry] The present embodiment uses a rotary drum dryer for drying, and high-temperature nitrogen is used as a heat source. The high-temperature nitrogen is introduced from the material discharge end of the rotary drum dryer and discharged from the material feeding end with organic vapor. During the rotation of the dryer drum, the polyphenylene ether particles are continuously introduced from one end of the dryer and the dried polyphenylene ether particles are continuously discharged from the other end. The rotation process of the drum realizes the transportation of the polyphenylene ether particles and the heat exchange with the hot nitrogen. The initial temperature T when the hot nitrogen is introduced in The outlet nitrogen temperature is 140-160°C. After heat exchange with polyphenylene ether particles to evaporate the solvent, the outlet nitrogen temperature is T out T r +20℃ to T r +40℃, where T r It is the boiling point of the main component of the washing liquid (methanol boiling point 64.5℃). The outlet nitrogen temperature is controlled within an appropriate range by introducing hot nitrogen. The outlet nitrogen temperature should not be too high or too low. If the outlet nitrogen temperature is too high, coking will easily occur and energy consumption will be high. If the outlet nitrogen temperature is too low, the polyphenylene ether will not be fully dried. The standard value for sufficient drying is set to a solvent content of less than or equal to 0.4%.
[0024] The method for producing polyphenylene ether particles of the present invention is not limited to the method for producing polyphenylene ether particles of the present embodiment described above, and the order, number of times, composition of washing liquid, drying section temperature, dryer form and structure, etc. of the specific operations in the above-mentioned polymerization process and post-treatment steps can be appropriately adjusted. Example
[0025] The present embodiment will be described in detail below with reference to specific examples and comparative examples thereof, but the present embodiment is not limited to the following examples.
[0026] [polymerization] Example
[0027] In a 3L double-layer glass reactor, add 1300g toluene, 12g aniline, 2g diethylamine, and 0.23g copper chloride. After stirring and dissolving, add 200g 2,6-dimethylphenol, adjust the material temperature to 30°C, and introduce oxygen from the bottom of the reactor under stirring conditions. The oxygen purity is 98.5% and the rate is 200mL / min to initiate polymerization. The material temperature is controlled between 40-43°C through the reactor jacket. After 60 minutes of polymerization, stop the oxygen and the polymerization is completed. Add 1.6g EDTA-2Na to the reactor to obtain a mixed solution of polyphenylene ether.
[0028] The mixed solution was mixed with 300 g of distilled water and allowed to stand for stratification, and the water layer was removed to obtain a polyphenylene ether solution P1. The weight average molecular weight obtained by sampling and testing was 18,500. Example
[0029] In a 3L double-layer glass reactor, add 1300g toluene, 12g aniline, 2g diethylamine, and 0.33g copper chloride. After stirring and dissolving, add 200g 2,6-dimethylphenol, adjust the material temperature to 30°C, and introduce oxygen from the bottom of the reactor under stirring conditions. The oxygen purity is 98.5% and the rate is 200mL / min to initiate polymerization. The material temperature is controlled between 40-43°C through the reactor jacket. After 60 minutes of polymerization, stop the oxygen and the polymerization is completed. Add 2g EDTA-2Na to the reactor to obtain a mixed solution of polyphenylene ether.
[0030] The mixed solution was mixed with 300 g of distilled water and allowed to stand for stratification, and the water layer was removed to obtain a polyphenylene ether solution P2. The weight average molecular weight obtained by sampling and testing was 29,000. Example
[0031] In a 3L double-layer glass reactor, add 1300g toluene, 12g aniline, 2g diethylamine, and 0.43g copper chloride. After stirring and dissolving, add 200g 2,6-dimethylphenol, adjust the material temperature to 30°C, and introduce oxygen from the bottom of the reactor under stirring conditions. The oxygen purity is 98.5% and the rate is 200mL / min to initiate polymerization. The material temperature is controlled between 40-43°C through the reactor jacket. After 60 minutes of polymerization, stop the oxygen and the polymerization is completed. Add 2g EDTA-2Na to the reactor to obtain a mixed solution of polyphenylene ether.
[0032] The mixed solution was mixed with 300 g of distilled water and allowed to stand for stratification, and the water layer was removed to obtain a polyphenylene ether solution P3. The weight average molecular weight obtained by sampling and testing was 48,000.
[0033] Comparative Example S1 In a 3L double-layer glass reactor, add 1300g toluene, 12g aniline, 2g diethylamine, and 0.13g copper chloride. After stirring and dissolving, add 200g 2,6-dimethylphenol, adjust the material temperature to 30°C, and introduce oxygen from the bottom of the reactor under stirring conditions. The oxygen purity is 98.5% and the rate is 200mL / min to initiate polymerization. The material temperature is controlled between 40-43°C through the reactor jacket. After 60 minutes of polymerization, stop the oxygen and the polymerization is completed. Add 2g EDTA-2Na to the reactor to obtain a mixed solution of polyphenylene ether.
[0034] The mixed solution was mixed with 300 g of distilled water and allowed to stand for stratification, and the water layer was removed to obtain a polyphenylene ether solution. The weight average molecular weight obtained by sampling and testing was 13,000. [Precipitation] Example
[0035] The polyphenylene ether solution P1 obtained in Example 1 was mixed with 1000 g of methanol and stirred at high speed for 10 minutes to obtain a slurry containing polyphenylene ether particles. After sampling and drying, the average diameter of the particles was measured to be 137 μm. Example
[0036] The polyphenylene ether solution P1 obtained in Example 1 was mixed with 1200 g of methanol and stirred at high speed for 10 minutes to obtain a slurry containing polyphenylene ether particles. After sampling and drying, the average diameter of the particles was measured to be 128 μm. Example
[0037] The polyphenylene ether solution P2 obtained in Example 2 was mixed with 1000 g of methanol and stirred at high speed for 10 minutes to obtain a slurry containing polyphenylene ether particles. After sampling and drying, the average diameter of the particles was measured to be 139 μm. Example
[0038] The polyphenylene ether solution P2 obtained in Example 2 was mixed with 1200 g of methanol and stirred at high speed for 10 minutes to obtain a slurry containing polyphenylene ether particles. After sampling and drying, the average diameter of the particles was measured to be 125 μm. Example
[0039] The polyphenylene ether solution P3 obtained in Example 3 was mixed with 1300 g of methanol and stirred at high speed for 10 minutes to obtain a slurry containing polyphenylene ether particles. After sampling and drying, the average diameter of the particles was measured to be 142 μm. Example
[0040] The polyphenylene ether solution P3 obtained in Example 3 was mixed with 1100 g of methanol and stirred at high speed for 10 minutes to obtain a slurry containing polyphenylene ether particles. After sampling and drying, the average diameter of the particles was measured to be 124 μm.
[0041] Comparative Example Y1 The polyphenylene ether solution P3 obtained in Example 3 was mixed with 3300 g of methanol and stirred at high speed for 10 minutes to obtain a slurry containing polyphenylene ether particles. After sampling and drying, the average diameter of the particles was measured to be 77 microns.
[0042] Comparative Example Y2 The polyphenylene ether solution obtained in Comparative Example S1 was mixed with 1000 g of methanol and stirred at high speed for 10 minutes to obtain a slurry containing polyphenylene ether particles. After sampling and drying, the average diameter of the particles was determined to be 93 μm. [Filtration and washing] Example
[0043] The polyphenylene ether particle slurry obtained in Example 4 was filtered, and the polyphenylene ether filter cake was washed with methanol washing liquid as washing liquid, the methanol washing liquid composition: 91.4% methanol, 8.2% water, 0.4% trimethylamine. The moisture content of the filter cake was 48%. Example
[0044] The polyphenylene ether particle slurry obtained in Example 5 was filtered, and the polyphenylene ether filter cake was washed with methanol washing liquid as washing liquid, the methanol washing liquid composition: 92% methanol, 7.5% water, 0.5% trimethylamine. The moisture content of the filter cake was 48%. Example
[0045] The polyphenylene ether particle slurry obtained in Example 6 was filtered, and the polyphenylene ether filter cake was washed with methanol washing liquid as washing liquid, the methanol washing liquid composition: 90.7% methanol, 9% water, 0.3% dimethylbutylamine. The moisture content of the filter cake was 47%. Example
[0046] The polyphenylene ether particle slurry obtained in Example 7 was filtered, and the polyphenylene ether filter cake was washed with methanol washing liquid as washing liquid, the methanol washing liquid composition: 93.8% methanol, 6% water, 0.6% trimethylamine. The moisture content of the filter cake was 46%. Example
[0047] The polyphenylene ether particle slurry obtained in Example 8 was filtered, and the polyphenylene ether filter cake was washed with a methanol washing solution, the composition of which was: 94.1% methanol, 5.5% water, and 0.4% trimethylamine. The moisture content of the filter cake was 47%. Example
[0048] The polyphenylene ether particle slurry obtained in Example 9 was filtered, and the polyphenylene ether filter cake was washed with methanol washing liquid as washing liquid, the methanol washing liquid composition: 91.4% methanol, 8.2% water, 0.4% dimethylbutylamine. The moisture content of the filter cake was 47%.
[0049] Comparative Example Z1 The polyphenylene ether particle slurry obtained in Example 9 was filtered, and the polyphenylene ether filter cake was washed with methanol washing liquid, the composition of the methanol washing liquid was: 91.8% methanol, 8.2% water. The moisture content of the filter cake was 48%.
[0050] Comparative Example Z2 The polyphenylene ether particle slurry obtained in Example 9 was filtered, and the polyphenylene ether filter cake was washed with methanol washing liquid as washing liquid, the methanol washing liquid composition: 99% methanol, 0.5% water, 0.5% trimethylamine. The moisture content of the filter cake was 52%.
[0051] Comparative Example Z3 The polyphenylene ether particle slurry obtained in Comparative Example Y1 was filtered, and the polyphenylene ether filter cake was washed with methanol washing liquid as washing liquid, the methanol washing liquid composition: 91.4% methanol, 8.2% water, 0.4% dimethylbutylamine. The moisture content of the filter cake was 47%. [dry] Example
[0052] The polyphenylene ether wet particles obtained in Example 10 were dried using a small rotary drum dryer with a rotation speed of 10 r / min, an initial hot nitrogen temperature of 145° C., a nitrogen exhaust temperature of 86° C., and an introduction rate of 12 L / min.
[0053] Results: There was no sticking or coking of the polyphenylene ether particles in the dryer, and the residual solvent content in the polyphenylene ether particles after drying was less than 0.4%. Example
[0054] The polyphenylene ether wet particles obtained in Example 11 were dried using a small rotary drum dryer with a rotation speed of 10 r / min, an initial hot nitrogen temperature of 145° C., a nitrogen exhaust temperature of 91° C., and an introduction rate of 14 L / min.
[0055] Results: There was no sticking or coking of the polyphenylene ether particles in the dryer, and the residual solvent content in the polyphenylene ether particles after drying was less than 0.4%. Example
[0056] The polyphenylene ether wet particles obtained in Example 12 were dried using a small rotary drum dryer with a rotation speed of 10 r / min, an initial hot nitrogen temperature of 155°C, a nitrogen exhaust temperature of 95°C, and an introduction rate of 12 L / min.
[0057] Results: There was no sticking or coking of the polyphenylene ether particles in the dryer, and the residual solvent content in the polyphenylene ether particles after drying was less than 0.4%. Example
[0058] The polyphenylene ether wet particles obtained in Example 13 were dried using a small rotary drum dryer with a rotation speed of 10 r / min, an initial hot nitrogen temperature of 155°C, a nitrogen exhaust temperature of 90°C, and an introduction rate of 10 L / min.
[0059] Results: There was no sticking or coking of the polyphenylene ether particles in the dryer, and the residual solvent content in the polyphenylene ether particles after drying was less than 0.4%. Example
[0060] The polyphenylene ether wet particles obtained in Example 14 were dried using a small rotary drum dryer with a rotation speed of 10 r / min, an initial hot nitrogen temperature of 160° C., a nitrogen exhaust temperature of 97° C., and an introduction rate of 10 L / min.
[0061] Results: There was no sticking or coking of the polyphenylene ether particles in the dryer, and the residual solvent content in the polyphenylene ether particles after drying was less than 0.4%. Example
[0062] The polyphenylene ether wet particles obtained in Example 15 were dried using a small rotary drum dryer with a rotation speed of 13 r / min, an initial hot nitrogen temperature of 155°C, a nitrogen exhaust temperature of 97°C, and an introduction rate of 10 L / min.
[0063] Results: There was no sticking or coking of the polyphenylene ether particles in the dryer, and the residual solvent content in the polyphenylene ether particles after drying was less than 0.4%.
[0064] Comparative Example Q1 The polyphenylene ether wet particles obtained in Example 15 were dried using a small rotary drum dryer with a rotation speed of 10 r / min, an initial hot nitrogen temperature of 130°C, a nitrogen exhaust temperature of 82°C, and an introduction rate of 10 L / min.
[0065] Results: The polyphenylene ether particles in the dryer were stuck together, and the residual solvent in the polyphenylene ether particles was greater than 0.9%, which did not meet the standard. The standard value is that the residual solvent is less than or equal to 0.4%.
[0066] Comparative Example Q2 The polyphenylene ether wet particles obtained in Example 15 were dried using a small rotary drum dryer with a rotation speed of 10 r / min, an initial hot nitrogen temperature of 170°C, a nitrogen exhaust temperature of 108°C, and an introduction rate of 10 L / min.
[0067] Result: A large area of coking occurred on the polyphenylene ether particles in the dryer, and the polyphenylene ether particles could not be smoothly discharged.
[0068] Comparative Example Q3 The polyphenylene ether wet particles obtained in Comparative Example Z1 were dried using a small rotary drum dryer with a rotation speed of 10 r / min, an initial temperature of hot nitrogen of 155° C., a nitrogen exhaust temperature of 89° C., and an introduction rate of 10 L / min.
[0069] Results: The polyphenylene ether particles in the dryer were sticky and attached to the inner wall of the dryer, and there was local coking.
[0070] Comparative Example Q4 The polyphenylene ether wet particles obtained in Comparative Example Z2 were dried using a small rotary drum dryer with a rotation speed of 10 r / min, an initial hot nitrogen temperature of 155° C., a nitrogen exhaust temperature of 89° C., and an introduction rate of 10 L / min.
[0071] Results: The polyphenylene ether particles in the dryer were sticky and adhered to the inner wall of the dryer.
[0072] Comparative Example Q5 The polyphenylene ether wet particles obtained in Comparative Example Z3 were dried using a small rotary drum dryer with a rotation speed of 10 r / min, an initial hot nitrogen temperature of 155° C., a nitrogen exhaust temperature of 89° C., and an introduction rate of 10 L / min.
[0073] Results: The polyphenylene ether particles in the dryer were stuck together and adhered to the inner wall of the dryer. During the process, polyphenylene ether powder flew up.
Claims
1. A method for producing polyphenylene ether particles, characterized in that: a) polymerization and precipitation process, using xylenol as a monomer, in the presence of a catalyst, an oxidative coupling reaction with oxygen in an organic solvent to obtain a polyphenylene ether mixed solution, the mixed solution is mixed with a poor solvent for precipitation, and the polyphenylene ether precipitated particles are controlled to have a suitable size by the ratio of the good solvent to the poor solvent; b) Filtration and washing process: when filtering and washing polyphenylene ether particles, the washing liquid contains poor solvents and washing accelerators; the moisture content of the filter cake is controlled after filtering and washing; c) Drying process: a rotary drum dryer is used for drying, and high temperature nitrogen is used as the heat source; The mass content of the bad solvent in the precipitation process is 40-50%, and the average particle size of the precipitated polyphenylene ether particles is greater than 120 microns; the washing liquid is mainly composed of the bad solvent of polyphenylene ether, preferably methanol; the washing accelerator includes water and dimethylamine, the water content is 5-10%, and the dimethylamine content is 0.1-2%; the moisture content of the filter cake after filtration and washing is less than 50%; during the drying process, high-temperature nitrogen is introduced from the material discharge end of the rotary drum dryer and discharged from the material addition end carrying organic vapor.
2. The polymerization and precipitation process according to claim 1, characterized in that The good solvent is an aromatic solvent such as xylene, chlorobenzene, toluene, etc.
3. The polymerization and precipitation process according to claim 1, characterized in that The poor solvent is an alcohol solvent such as methanol, propylene glycol, ethanol, butanol, etc.
4. The filtering and washing process according to claim 1, characterized in that The lotion composition contains water, wherein the water content is 5-10%.
5. The filtering and washing process according to claim 1, characterized in that The washing liquid composition has a dimethylamine compound of structure (CH3)2NX, wherein X is C 1-10 The alkyl substituent has a dimethylamine compound content of 0.1-2%.
6. The drying method according to claim 1, characterized in that: Initial temperature T when high temperature nitrogen is introduced into the dryer in The outlet nitrogen temperature is 140-160℃. After heat exchange with polyphenylene ether particles to evaporate the solvent, the outlet nitrogen temperature is T out T r +20℃ to T r +40℃, where T r It is the boiling point of the main component of the lotion.
7. The polyphenylene ether according to claim 1, characterized in that The weight average molecular weight of the polyphenylene ether is greater than 15,000.
Citation Information
Patent Citations
Method for producing polyphenylene ether
CN107236124A
Polyphenylene ether powder and production method
CN108017791A
Method for producing polyphenylene ether
CN111978535A
Polyphenyl ether powder and preparation method thereof
CN117024786A
Method for producing polyphenylene ether
JP2020193320A