Recycling method of coal chemical solid waste

After mixing coal chemical sludge and gasified fine slag filter cake, the dry slag is dehydrated by using a super-strong filter press to produce dry slag and incinerate it in the boiler, the high moisture content and complex components in the recycling and utilization of coal chemical solid waste are solved. The problem has achieved low-cost and efficient combustion and resource recycling.

CN118978311APending Publication Date: 2024-11-19SICHUAN NORMAL UNIV LVHUAN BIOTECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411234027.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Gasified fine slag filter cakes and sludge produced in the coal chemical industry are difficult to recycle due to high moisture content and complex components. The existing methods to reduce moisture content are inefficient or costly, which limit their recycling as low-calorie fuels. use.

Method used

Mix sludge with a moisture content of no less than 75% and a gasified fine slag filter cake with a moisture content of 40% to 60% at a mass ratio of 1:1 to 10, and press and dehydrate through a super-strong filter press to obtain a moisture content of 30%. ~35% of the dry slag was incinerated in the boiler to collect the ash for recycling.

Benefits of technology

The low-cost and efficient dehydration of gasified fine slag and sludge is achieved, the combustion conditions are met, and the recycling costs are reduced. The ash obtained after incineration can be used in the fields of building materials and other fields, realizing the comprehensive utilization of resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978311A_ABST
    Figure CN118978311A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of solid waste recycling, and particularly discloses a coal chemical industry solid waste recycling method which comprises the following steps: 1) uniformly mixing and stirring sludge with the water content of not less than 75% and a gasified fine slag filter cake with the water content of 40-60% in the coal chemical industry production process according to the mass ratio of 1: (1-10) to obtain a mixture; (2) squeezing and dehydrating the mixture to prepare dry slag with the water content of 30-35%; (3) the dried slag is incinerated through a boiler, and heat generated by complete combustion of the dried slag is recycled; and 4) collecting ash after the dry slag is burnt out, and recycling for later use. The characteristics of the sludge and the gasified fine slag are fully utilized, the sludge and the gasified fine slag are mixed and squeezed to prepare the dried slag, the technical bottlenecks that the gasified fine slag and the sludge are high in moisture and difficult to dehydrate are broken through, the difficulty of recycling the gasified fine slag and the sludge is overcome, combustion heat can be provided, inorganic ash with relatively simple components can be obtained, low-cost recycling of the gasified fine slag and the sludge is achieved, and the method is suitable for industrial production. And the method is suitable for being widely popularized and applied in coal chemical fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid waste recycling, and in particular to a method for recycling coal chemical solid waste. Background Art

[0002] A major transformation in the development of the coal industry in the past 20 years is to vigorously develop the modern coal chemical industry, partially replacing the petrochemical industry that uses oil as raw materials. Coal chemical industry mainly includes coal gasification, liquefaction, distillation, tar processing and calcium carbide acetylene chemical industry. With the continuous reduction of world oil resources, coal chemical industry has broad prospects. Coal gasification occupies an important position in coal chemical industry. It is used to produce various gas fuels. It is a clean energy source and is beneficial to environmental protection. The product of coal gasification, synthesis gas, is the raw material for manufacturing liquid fuels, synthetic ammonia, urea, methanol, ethylene glycol and other chemical products.

[0003] Gasification fine slag is a solid waste that is inevitably generated during the coal gasification process. The main disposal methods for gasification fine slag are landfill or stockpiling. Sludge is another type of solid waste generated during the treatment of coal chemical wastewater. Due to the high water content of sludge, it is extremely difficult to dehydrate, and a large amount of conditioning agents are added to the sludge, resulting in a complex composition of coal chemical sludge. It can neither be used as a raw material for the production of other products nor as a low calorific value fuel. It is basically impossible to recycle and can only be disposed of by landfill. Among the coal chemical solid wastes, the gasification fine slag filter cake with a moisture content of about 60% and the sludge with a moisture content of about 80% are more difficult to handle than other solid wastes.

[0004] The gasification fine slag filter cake is a solid waste after the crude synthesis gas is washed and the washing wastewater (also called black water) is flocculated and vacuum filtered. The gasification fine slag filter cake has developed internal voids and a lot of water adsorbed on the inner surface. It is usually within 180μm in particle size, sticky, with a residual carbon content of 20-50% (dry basis) and a calorific value of 2000-3000kcal / kg. Although the dry basis residual carbon and calorific value are high, the water will absorb heat and vaporize first during the combustion process. If the moisture content is not reduced, the residual carbon calorific value is not enough to maintain its own combustion. Therefore, the moisture content must be reduced in order to recycle the gasification fine slag. The existing methods for reducing the moisture content of the gasification fine slag filter cake are either to flatten the gasification fine slag filter cake in a large space and dry it, or to dry it through other heat media. The drying process occupies a large area, cannot be exposed to the open air, and has low efficiency. The drying cost is high. These measures limit the recycling of gasification fine slag as a low calorific value fuel. In addition, the particle size of the gasification fine slag filter cake is too small, and ordinary boilers cannot burn the gasification fine slag filter cake with too small a particle size, so the boiler needs to be modified, which also increases the cost and limits the recycling of the gasification fine slag. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention aims to provide a method for recycling coal chemical solid waste.

[0006] In order to achieve the above object, the present invention is implemented by the following technical scheme: a method for recycling coal chemical solid waste, comprising the following steps:

[0007] (1) Sludge with a moisture content of not less than 75% produced in the coal chemical production process and gasification fine slag filter cake with a moisture content of 40% to 60% are mixed and stirred in a mass ratio of 1:1 to 10 to obtain a mixture;

[0008] (2) squeezing and dehydrating the mixture to obtain dried slag with a moisture content of 30% to 35%;

[0009] (3) Using a boiler to burn the dried slag to completely burn the dried slag and recover the heat generated by the combustion;

[0010] (4) Collect the ash left after the dried slag is completely burned and recycle it for later use.

[0011] This technical solution is mainly aimed at recycling the sludge and gasification fine residue generated in the production process of the coal chemical industry.

[0012] The water content of sludge produced by coal chemical industry reaches 80%. General filter press equipment or dehydration equipment cannot dehydrate sludge with such high water content. Therefore, it is necessary to add conditioning agents to reduce the water content of sludge. In addition, the composition of sludge in coal chemical industry is complex. In order to avoid polluting the environment after landfill, it is also necessary to add agents for oxidation and decontamination (mainly to remove halogen ions), which also leads to limited application of sludge. In addition, sludge has basically no calorific value. If the sludge is incinerated according to the routine, it is necessary to add additional fuel coal to achieve it. The ash left after incineration can be used as a raw material for building materials such as bricks and cement. Therefore, to achieve the recycling of sludge, two conditions must be met: first, reduce the water content of sludge, and second, incinerate the sludge. These two processes undoubtedly increase the cost of sludge recycling and limit the recycling of sludge. Based on the cost required for the above two conditions, at present, coal chemical sludge is only directly landfilled after adding agents for oxidation and decontamination, and is not recycled.

[0013] The gasification fine slag filter cake produced by coal chemical industry comes from the wastewater used to wash the flue gas. After the washing wastewater is flocculated and vacuum filtered, the solid substance obtained is the gasification fine slag filter cake. The moisture content of the gasification fine slag filter cake is 40% to 60%, and it has a high residual carbon content, so it has a certain calorific value and can be used as a low calorific value fuel. However, the moisture content of the gasification fine slag filter cake with a moisture content of 40% to 60% will first absorb heat and vaporize during the combustion process. If the moisture content is not reduced, the residual carbon calorific value is not enough to maintain its own combustion, that is, it cannot be self-stabilized in the boiler. The gasification fine slag filter cake with a high moisture content has a large viscosity and cannot be mixed evenly with the fuel coal, so that the blending combustion cannot be achieved. In addition, the gasification fine slag filter cake has a high residual carbon content and a large loss on ignition, and it cannot be used directly as a raw material for brick making. Therefore, if the gasification fine slag is to be recycled as a low calorific value fuel, its moisture content must be further reduced. There are two main methods to reduce the gasification fine slag filter cake. One is to spread it over a large area and dry it in the sun, and the other is to use a high-heat medium to dry it. Since the particle size of the gasification fine slag filter cake is extremely small and the internal pores are well-developed, it is very easy to absorb water. The gasification fine slag filter cake cannot be spread out in the open air and the spreading area cannot be small, and the drying efficiency is extremely low. Due to its small particle size, it must be protected from wind after drying, otherwise it is very easy to generate dust and pollute the environment. The cost of using a high-heat medium to dry the gasification fine slag filter cake is extremely high. Also, because the particle size of the gasification fine slag filter cake is extremely small, secondary combustion (afterburning) will occur in the flue at the tail of the boiler. Therefore, the gasification fine slag filter cake cannot be burned in a general boiler, and the boiler needs to be modified, which also increases the cost of recycling the gasification fine slag as a low calorific value fuel. Based on the above reasons, recycling gasification fine slag as low calorific value fuel also needs to meet two conditions: first, low-cost and high-efficiency dehydration of gasification fine slag filter cake to reduce its moisture content so that it meets the fuel standard; second, adding a binder to the gasification fine slag filter cake to increase its particle size so that it can meet the conditions for combustion in general boilers.

[0014] This technical solution mixes sludge with a moisture content of not less than 75% with gasification fine slag filter cake with a moisture content of 40% to 60%. The moisture content of the obtained mixture meets the requirements of the super filter press feed, and can be squeezed and dehydrated by the super filter press to obtain dried slag with a moisture content of 30% to 35%. The dried slag is loose and non-sticky, and is easy to mix evenly with fuel coal to meet the combustion conditions. Gasification fine slag and sludge are solid wastes, and the cost of mixing and further squeezing and dehydrating the two is very low. They have a certain calorific value and meet the two conditions for sludge recycling. In addition, coal chemical sludge contains a certain amount of organic matter and water treatment flocculant, which can be used as a binder for gasification fine slag filter cake, increase the particle size of the dried slag, so that it can be burned in a general boiler, and meet the conditions of gasification fine slag as a low calorific value fuel.

[0015] When the dried slag is burned in a general boiler, the gasified fine slag is used as a low calorific value fuel to provide heat, and the heat generated can be recycled. After the sludge is burned, the complex components and organic matter inside it are oxidized, leaving only simple inorganic ash, which can be recycled. The comprehensive utilization of ash includes cement, building materials, roadbed, soil corrective agent, water treatment agent and other aspects.

[0016] In order to better implement the method of the present invention, further, in the step (1), the mixture is prepared by mixing and stirring sludge with a moisture content of not less than 80% and gasification fine residue filter cake with a moisture content of 45% to 60% in a mass ratio of 1:2.

[0017] In order to better implement the method of the present invention, further, in the step (2), an ultra-strong filter press is used to squeeze and dehydrate the mixture.

[0018] In order to better implement the method of the present invention, further, the ultra-strong filter press includes a frame, a conveying device and a pressing device. A collecting trough is arranged in the frame, the conveying device is arranged on the frame and located above the collecting trough, the two ends of the conveying device are respectively connected to the two ends of the frame, and the two ends of the conveying device extend out of the two ends of the frame respectively, and the pressing device is arranged above the conveying device, and the pressing device is used to press and dehydrate the mixture of sludge and gasified fine slag filter cake conveyed on the conveying device.

[0019] In order to better implement the method of the present invention, further, the main operating parameters of the ultra-strong filter press include:

[0020] Amount of mixture of sludge and gasification fine residue cake treated by a single machine: 10t / h;

[0021] Design pressure: 80kg / cm 2 ;

[0022] Working pressure acting on the mixture of sludge and gasification fine residue filter cake: 50~60kg / cm 2 ;

[0023] Filter pressing time: 180s;

[0024] Power: 125kw.

[0025] In order to better implement the method of the present invention, further, in the step (3), the main process of using a boiler to incinerate the dried slag is to reduce the moisture content of the dried slag to 30% to 35% and mix it with fuel coal, and then add them into the boiler for incineration, wherein the mass fraction of the dried slag mixed is not more than 20%.

[0026] In order to better implement the method of the present invention, further, in the step (1), the sludge with a moisture content of not less than 80% and the gasification fine residue filter cake with a moisture content of 45% to 60% are initially stored in a sludge storage tank and a storage bin respectively, the sludge in the sludge storage tank and the gasification fine residue filter cake in the storage bin are mixed in the sludge conditioning reactor, the sludge with a moisture content of not less than 80% is injected from the sludge storage tank into the sludge conditioning reactor through a sludge injection pump, and the gasification fine residue filter cake with a moisture content of 45% to 60% is injected from the storage bin into the sludge conditioning reactor through a paste pump.

[0027] In order to better implement the method of the present invention, further, in the step (4), the collected ash can be recycled as a raw material for preparing building materials; the prepared building materials include fly ash bricks, fly ash ceramics, and hollow bricks.

[0028] In order to better implement the method of the present invention, further, in the step (4), the collected ash can also be recycled as an admixture for preparing cement.

[0029] In order to better implement the method of the present invention, further, in the step (4), the collected ash can also be recycled as a raw material for preparing fertilizer or a soil conditioner.

[0030] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0031] (1) The present invention realizes the recycling of gasification fine slag by using gasification fine slag filter cake as a low calorific value fuel to provide heat. The sludge is used as a binder for the gasification fine slag filter cake, which increases the particle size of the gasification fine slag filter cake, so that it can be used as fuel by ordinary boilers, thereby realizing stable operation of the boiler without the need to modify the boiler, and reducing the recovery cost of the gasification fine slag;

[0032] (2) The present invention uses gasified fine slag as fuel for incinerating sludge, without the need to use additional fuel coal, and can effectively remove complex components and organic matter in the sludge, leaving only inorganic ash with relatively simple components, thus realizing not only the disposal process of the sludge, but also the recycling of the sludge, and the cost is extremely low;

[0033] (3) The present invention uses an ultra-strong filter press to squeeze and dehydrate the mixture of gasification fine slag filter cake and sludge, and can obtain dried slag with a moisture content of 30% to 35%, so that the dried slag meets the combustion standard. Compared with the existing dehydration method of gasification fine slag filter cake and sludge, the dehydration method is low in cost and high in efficiency;

[0034] (4) The recovery method provided by the present invention makes full use of the characteristics of sludge and gasification fine residue filter cake, and makes the dried slag obtained by mixing and squeezing the two, breaking the technical bottleneck of high moisture content and difficult dehydration of gasification fine residue filter cake and sludge, and overcoming the difficulties in recycling the two. It can not only provide combustion heat, but also obtain inorganic ash with relatively simple composition, perfectly recycle the two at low cost, and minimize the consumption of fuel coal. It is suitable for wide promotion and application in coal chemical industry. The gasification fine residue and sludge of coal chemical industry are both general solid wastes. Coordinated disposal and resource utilization in the factory can promote the high-quality development of coal chemical enterprises. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments with reference to the following drawings:

[0036] Figure 1 is a flow chart of the method of the present invention;

[0037] Figure 2 This is a test diagram of the state of the gasified fine residue filter cake and sludge before pressing and the moisture content in the present invention;

[0038] Figure 3 The state of the mixture obtained by mixing the sludge and the gasification fine residue filter cake in a mass ratio of 1:2 before pressing and the moisture content test diagram in the present invention;

[0039] Figure 4 The diagram shows the states of two groups of mixtures after being squeezed and the moisture content test diagram in the present invention. DETAILED DESCRIPTION

[0040] In order to make the purpose, process conditions and advantages of the present invention more clearly understood, the present invention is further described in detail in conjunction with the following embodiments, but the embodiments of the present invention are not limited thereto. Without departing from the above-mentioned technical ideas of the present invention, various substitutions and changes are made according to the common technical knowledge and customary means in the field, which should all be included in the scope of the present invention. The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0041] Embodiment 1:

[0042] This embodiment provides a method for recycling coal chemical solid waste, the specific process is as follows: Figure 1 As shown, the details are as follows:

[0043] (1) Transporting sludge with a moisture content of not less than 75% produced by coal chemical industry to a sludge storage tank for storage by means of vehicle or pipeline transportation;

[0044] (2) using a conveyor belt to convey the gasified fine slag filter cake that has been preliminarily dehydrated by the vacuum filter to a storage bin for storage;

[0045] (3) The sludge is injected from the sludge storage tank into the sludge conditioning reactor through a sludge injection pump, and the gasification fine residue filter cake is injected from the storage bin into the sludge conditioning reactor through a paste pump, and the sludge and the gasification fine residue filter cake are stirred and mixed uniformly through the sludge conditioning reactor to obtain a mixture;

[0046] (4) The mixture in the sludge conditioning reactor is conveyed to an ultra-strong filter press by a screw conveyor, and is squeezed and dehydrated by the ultra-strong filter press. The resulting squeezed liquid is conveyed to a water pool for treatment and reuse, and the obtained dried slag is transported to a coal blending station by a transport vehicle;

[0047] (5) Mixing fuel coal with dried slag in a coal blending station and finally transporting them to a boiler for combustion, wherein the mass percentage of the dried slag mixed does not exceed 20%;

[0048] (6) Recover and utilize the heat generated by the boiler, and recover the ash remaining after the dry slag mixed with the fuel coal is completely burned for future use.

[0049] Embodiment 2:

[0050] Based on the above embodiments, this embodiment further limits the squeezing process of the mixture by the ultra-strong filter press. The ultra-strong filter press can reduce the moisture content of the sludge to an extremely low level. After the sludge is mixed with the gasified fine slag filter cake, the moisture content of the sludge is reduced, meeting the feeding conditions of the ultra-strong filter press.

[0051] The gasification fine slag filter cake with a moisture content of 45% to 60% can also be directly squeezed and dehydrated by the super filter press. The moisture content of the gasification fine slag dried slag after squeezing is 30% to 35%. Therefore, after the gasification fine slag filter cake is mixed with the sludge, although the moisture content of the mixture is slightly higher than that of the gasification fine slag filter cake, it does not affect the squeezing and dehydration process of the mixture using the super filter press.

[0052] Among them, the ultra-strong filter press includes a frame, a conveying device and a pressing device. A collecting trough is arranged in the frame. The conveying device is arranged on the frame and located above the collecting trough. The two ends of the conveying device are respectively connected to the two ends of the frame, and the two ends of the conveying device extend out of the two ends of the frame respectively. The pressing device is arranged above the conveying device, and the pressing device is used to press and dehydrate the mixture of sludge and gasified fine slag filter cake conveyed on the conveying device.

[0053] The main working parameters of the super filter press include:

[0054] Amount of mixture of sludge and gasification fine residue filter cake treated by a single machine: 10t / h;

[0055] Design pressure: 80kg / cm2 ;

[0056] Working pressure acting on the mixture of sludge and gasification fine residue filter cake: 50~60kg / cm 2 ;

[0057] Filter pressing time: 180s;

[0058] Power: 125kw.

[0059] The specific structure of the ultra-strong filter press has been applied for an invention patent, with the application number 202010587504.3, and has been disclosed. It belongs to the prior art and will not be elaborated here.

[0060] Embodiment 3:

[0061] This embodiment provides a specific squeezing example based on the above embodiment, which is as follows:

[0062] Gasification fine residue filter cake and sludge that are not squeezed by super filter press, such as Figure 2 As shown, the moisture content of the gasification fine slag filter cake is 42.67%, and the moisture content of the sludge is 79.60%.

[0063] The gasification fine residue filter cake and sludge were squeezed separately using a super filter press, and then industrial analysis was performed on both. The specific situation is shown in Table 1:

[0064] Table 1 Industrial analysis of gasification fine residue filter cake and sludge after pressing

[0065] name Gasification fine slag sludge Total water Mt (%) 27.05 51.54 Internal water Mad(%) 0.32 3.53 Air-dry basis total sulfur St, ad (%) 1.31 0.45 Air dried basis ash content Aad (%) 60.24 67.96 Volatile matter Vad (%) 1.04 27.74 Fixed carbon FCad (%) 38.4 0.77 Received basic lower calorific value Qnet.ar (Kcal / kg) 2030 / Dry basis higher calorific value Qgr.d (Kcal / kg) 3016 /

[0066] According to Table 1, the calorific value of the gasified fine slag filter cake is significantly improved after being squeezed and dehydrated by the ultra-strong filter press, and it can be used as a low calorific value fuel. However, the calorific value of the sludge after being squeezed and dehydrated by the ultra-strong filter press cannot be detected because it does not meet the minimum measurement standard and cannot be burned as fuel.

[0067] Embodiment 4:

[0068] Based on the above embodiments, this embodiment explores the optimal mass ratio of gasification fine slag filter cake and sludge, and the specific process is as follows:

[0069] The percentage of sludge and gasification fine residue filter cake in the mixture was adjusted, and the mixture was grouped according to the percentage content. After the mixture of each group was squeezed and dehydrated by a super filter press, the two were industrially analyzed. The specific situation is shown in Table 2:

[0070] Table 2 Industrial analysis values ​​of mixtures with different raw material ratios after pressing

[0071]

[0072] According to Table 2, the higher the sludge content, the lower the calorific value of the mixture, and the higher the moisture content after squeezing. In theory, the addition of sludge is not good for the overall industrial analysis value of the gasification fine slag filter cake. However, since the present invention needs to dispose of the sludge, and the combustion of the gasification fine slag filter cake requires sludge as a binder, after comprehensive consideration, the ratio of the second group is selected as the optimal ratio of sludge and gasification fine slag filter cake. That is, the mass ratio of sludge to gasification fine slag filter cake is 1:2.

[0073] The sludge and gasification fine residue filter cake were mixed in a mass ratio of 1:2, and the moisture content of the mixture was tested before being squeezed and dehydrated by the super filter press. Figure 3 As shown, the moisture content of the mixture is 54.03%, which is basically consistent with the calculated moisture content value of 54.98%.

[0074] The obtained mixture was divided into two groups, and dried slag was obtained after being squeezed. The moisture content of the dried slag of the first group was 30.59%, and the moisture content of the dried slag of the second group was 28.59%. The average value of the two groups, 29.59%, was taken as the moisture content of the mixture after squeezing and dehydration. Figure 4 shown.

[0075] Embodiment 5:

[0076] Based on the above embodiment, this embodiment further defines the use of the ash after the dry slag is completely burned. Landfill is the traditional way to deal with sludge produced by coal chemical industry. However, the sludge contains toxic substances. As landfill material, it will pollute groundwater, thus posing a potential threat to the environment and people's health. The ash finally obtained by burning sludge is used as building backfill, filling low-lying land and wasteland, filling mines, etc. The residual toxic substances are oxidized or passivated during the incineration process, and even if it is landfilled, it will not cause groundwater and soil pollution.

[0077] In addition, the collected ash can be recycled as a raw material for preparing building materials; the prepared building materials include fly ash bricks, fly ash ceramics, and hollow bricks. Since the sludge has complex components and contains a certain amount of organic matter, if it is directly used as a raw material for brick making, it will emit odorous gases during the process of making and firing, which will also have a great impact on the quality of the bricks. Therefore, the sludge cannot be directly used as a raw material for brick making. Using the ash after combustion as a raw material for brick making can turn waste into treasure.

[0078] The collected ash can also be recycled as an admixture for preparing cement, a raw material for preparing fertilizers or a soil conditioner. The mixture of sludge and gasification fine slag filter cake at a mass ratio of 1:2 is squeezed by a super filter press to obtain dried slag. The mass percentage of the dried slag and fuel coal is 20%, and they are added to the boiler for incineration to make the dried slag completely burn, recover the heat generated by the combustion, collect the ash left after the dried slag is completely burned, and conduct chemical composition analysis, which is compared with the fly ash composition obtained by the complete combustion of fuel coal. The specific situation is shown in Table 3:

[0079] Table 3 Analysis of ash components of dried slag and fuel coal after complete combustion

[0080]

[0081]

[0082] According to Table 3, the ash left after the complete combustion of the dried slag is basically the same in chemical composition as the fly ash obtained by the complete combustion of the fuel coal. Therefore, the collected ash is recycled as an admixture for preparing cement and a raw material for preparing fertilizers or a soil conditioner, which meets the quality requirements of fly ash used in cement and concrete.

[0083] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.

Claims

1. A method for recycling coal chemical solid waste, characterized in that: The following steps are involved: (1) Sludge with a moisture content of not less than 75% produced in the coal chemical production process and gasification fine slag filter cake with a moisture content of 40% to 60% are mixed and stirred evenly in a mass ratio of 1:1 to 10 to obtain a mixture; (2) Pressing and dehydrating the mixture to obtain dried slag with a moisture content of 30% to 35%; (3) Use a boiler to burn the dried slag to ensure complete combustion of the dried slag and recover the heat generated by the combustion; (4) Collect the ash left after the dried slag is completely burned and recycle it for later use.

2. The method for recycling coal chemical solid waste according to claim 1, characterized in that: In the step (1), the mixture is prepared by mixing and stirring sludge having a moisture content of not less than 80% and gasification fine residue filter cake having a moisture content of 45% to 60% in a mass ratio of 1:

2.

3. A method for recycling coal chemical solid waste according to claim 1 or 2, characterized in that: In the step (2), the mixture is squeezed and dehydrated using an ultra-strong filter press.

4. The method for recycling coal chemical solid waste according to claim 3, characterized in that: The ultra-strong filter press includes a frame, a conveying device and a pressing device. A collecting trough is arranged in the frame. The conveying device is arranged on the frame and located above the collecting trough. Two ends of the conveying device are respectively connected to two ends of the frame, and the two ends of the conveying device extend out of two ends of the frame respectively. The pressing device is arranged above the conveying device, and the pressing device is used to press and dehydrate the mixture of sludge and gasified fine slag filter cake conveyed on the conveying device.

5. The method for recycling coal chemical solid waste according to claim 4, characterized in that: The main working parameters of the super filter press include: Amount of mixture of sludge and gasification fine residue cake treated by a single machine: 10t / h; Design pressure: 80kg / cm 2 ; Working pressure acting on the mixture of sludge and gasification fine residue filter cake: 50~60 kg / cm 2 ; Filter pressing time: 180s; Power: 125kw.

6. A method for recycling coal chemical solid waste according to claim 1 or 2, characterized in that: In step (3), the main process of using a boiler to incinerate the dried slag is to reduce the moisture content of the dried slag to 30% to 35% and mix it with fuel coal, and then add them into the boiler for incineration, wherein the mass fraction of the dried slag mixed is not more than 20%.

7. A method for recycling coal chemical solid waste according to claim 1 or 2, characterized in that: In the step (1), the sludge with a moisture content of not less than 80% and the gasification fine residue filter cake with a moisture content of 45% to 60% are initially stored in a sludge storage tank and a storage bin, respectively. The sludge in the sludge storage tank and the gasification fine residue filter cake in the storage bin are mixed in a sludge conditioning reactor. The sludge with a moisture content of not less than 80% is injected from the sludge storage tank into the sludge conditioning reactor by a sludge injection pump, and the gasification fine residue filter cake with a moisture content of 45% to 60% is injected from the storage bin into the sludge conditioning reactor by a paste pump.

8. A method for recycling coal chemical solid waste according to claim 1 or 2, characterized in that: In the step (4), the collected ash can be recycled as a raw material for preparing building materials; the prepared building materials include fly ash bricks, fly ash ceramics, and hollow bricks.

9. A method for recycling coal chemical solid waste according to claim 1 or 2, characterized in that: In the step (4), the collected ash can also be recycled as an admixture for preparing cement.

10. A method for recycling coal chemical solid waste according to claim 1 or 2, characterized in that: In step (4), the collected ash can also be recycled as a raw material for preparing fertilizer or a soil conditioner.

Citation Information

Patent Citations

  • Powerful squeezing sludge dewatering device

    CN111620535A

  • Process and device for improving filter pressing performance of tail coal slime with coal gasification fine slag

    CN110790469A

  • Municipal sludge and gasified slag cooperative treatment method

    CN114702218A

  • Cooperative treatment method for gasified slag, sludge and low-value coal slime

    CN116590024A

  • Deep dehydration method for coal chemical gasification fine slag

    CN117505475A