Modified polypropylene film, preparation method thereof and polypropylene-based photovoltaic backboard

Through the hot press fusion technology of modified polypropylene film and continuous fiber reinforced polypropylene composite materials, the prone to cracking and aging of traditional photovoltaic backplanes under humid and heat conditions is solved, the weather resistance and environmental protection are improved, and the photovoltaic modules are ensured. Long-term reliability and environmental protection.

CN118978782APending Publication Date: 2024-11-19JIANGSU QIYI TECH +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411098536.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Traditional photovoltaic back panels are prone to cracking and delamination under humid and heat conditions, have poor weather resistance and water vapor barrier resistance, and the fluorine film contaminates the environment and the adhesive layer is prone to aging, resulting in reduced efficiency or failure of photovoltaic modules.

Method used

Modified polypropylene film and continuous fiber reinforced polypropylene composite material are used to fusion molding through hot pressing, combining the UV shielding function of alkyl compounds and nano-level physical shielding agents to improve the UV resistance and mechanical properties of the back plate.

Benefits of technology

It significantly enhances the weather resistance and environmental protection of the photovoltaic backplane, avoids the aging of the bonding layer, and ensures the reliability and environmental protection of long-term use of photovoltaic modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978782A_ABST
    Figure CN118978782A_ABST
Patent Text Reader

Abstract

The embodiment of the invention provides a modified polypropylene film, a preparation method thereof and a polypropylene-based photovoltaic backplane, the modified polypropylene film comprises the following components by weight: 100 parts of polypropylene; 0.01 to 0.1 part of an initiator; 0.1 to 3 parts of a silane compound; 5 to 50 parts of UV shielding nano powder; and 1 part of an antioxidant. The modified polypropylene film provided by the scheme is high in ultraviolet resistance and relatively high in mechanical properties such as tensile property, tearing property and the like. According to the polypropylene-based photovoltaic backboard provided by the scheme, the inner layer and the outer layer both select environment-friendly polypropylene as a polymer base material and are molded through hot-pressing fusion, so that the risk that a bonding layer of a traditional photovoltaic backboard is easy to age, peel and fall off is eliminated from the source, and the reliability and the environmental protection property of a photovoltaic backboard assembly in long-term use are ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of photovoltaic backplanes, and in particular to a modified polypropylene film, a preparation method thereof, and a polypropylene-based photovoltaic backplane. Background Art

[0002] The photovoltaic module backsheet is a packaging material used for solar cell modules and is located on the outermost layer on the back of the solar cell module. In order to keep the solar cell service life longer, the photovoltaic backsheet should have reliable mechanical properties, electrical insulation, excellent high and low temperature resistance, water vapor barrier and UV aging resistance.

[0003] The current mainstream photovoltaic backplane is a multi-layer composite structure, including a substrate layer, a protective layer and an adhesive layer. The substrate layer is mainly a PET (Polyethylene terephthalate) layer, and the protective layer is mainly a fluorine film. However, PET materials are prone to cracking and delamination under hot and humid conditions, and their adhesion is reduced, and their weather resistance and water vapor barrier properties are poor. Although the fluorine film can provide weather resistance, wear resistance, flame retardancy, water resistance, etc. for the backplane, it is difficult to degrade and easily pollutes the environment. At the same time, there is a risk of aging of the adhesive layer, which leads to the peeling of the film material, thereby significantly reducing the efficiency of the photovoltaic module or even causing failure. Therefore, the research and development of fluorine-free high-performance photovoltaic backplanes has great application value.

[0004] Polyolefin materials can make up for these shortcomings of traditional photovoltaic backsheets after modification and processing, and have better water vapor barrier resistance than PET. Therefore, using polyolefin materials to completely or partially replace fluorine film and / or PET substrate to obtain a more environmentally friendly photovoltaic backsheet, while improving the weather resistance and water vapor barrier resistance of the backsheet, is currently a major development and application direction of photovoltaic backsheets.

[0005] Polypropylene (PP for short) is a semi-crystalline polyolefin thermoplastic. It has high impact resistance, strong mechanical properties, and resistance to corrosion by a variety of organic solvents and acids and alkalis. Its relative density is small, only 0.89-0.91, and it is one of the lightest varieties of plastics. Continuous glass fiber reinforced polypropylene composite materials are the preferred substrate for preparing fluorine-free backsheets because of their excellent properties such as strong impact resistance, excellent designability, recyclability, and low cost. A large number of studies have shown that sunlight, especially ultraviolet rays with shorter wavelengths, can cut off the molecular chain of PP and induce photooxidation of PP under the action of oxygen. The most sensitive wavelength of PP is 300nm, resulting in very poor resistance to photooxidation aging of PP. The photooxidation aging of PP is carried out in a manner similar to a free radical chain reaction. After aging, carbonyl compounds will be produced, and carbonyl groups can absorb ultraviolet light of 260-340nm and participate in a variety of complex photochemical reactions, thereby causing the PP molecular chain to break, which is prone to photooxidation aging and degradation. This drawback restricts the long-term and stable application of PP in photovoltaic backsheets in open-air environments. However, studies have shown that its anti-aging performance can be greatly improved through weathering modification.

[0006] UV (Ultraviolet) shielding agents are divided into two categories: physical shielding agents and chemical shielding agents. The mechanism of action of physical shielding agents is mainly to reflect and scatter ultraviolet rays. Typical representatives include titanium dioxide, zinc oxide, carbon black, etc. Chemical shielding agents can absorb ultraviolet rays. In organic molecules, functional groups with specific structural characteristics usually lead to strong absorption in the ultraviolet light region (200 to 400 nanometer wavelength range). For example, aromatic compounds, olefin functional groups with double or triple bonds, and carbene compounds with carbon-oxygen double bonds, such as ketones and aldehydes. Summary of the invention

[0007] The main purpose of the present application is to provide a modified polypropylene film, a preparation method thereof and a polypropylene-based photovoltaic backsheet, so as to solve the problem that the traditional photovoltaic backsheet is not very environmentally friendly and the adhesive layer is prone to aging and falling off.

[0008] To achieve the above-mentioned object, the first aspect of the present application provides a modified polypropylene film, which comprises the following components in parts by weight:

[0009] Polypropylene 100 parts;

[0010] Initiator 0.01-0.1 part;

[0011] Silane compound 0.1-3 parts;

[0012] 5-50 parts of UV shielding nano powder;

[0013] 1 part antioxidant.

[0014] In one embodiment, the initiator is a peroxide initiator or an azo initiator.

[0015] In one embodiment, the silane compound comprises a vinyl group, a UV shielding functional group and a hydrolyzable functional group.

[0016] In one embodiment, the UV shielding nano powder is selected from at least one of nano titanium dioxide and nano zinc oxide.

[0017] In one embodiment, the antioxidant is selected from at least one of antioxidant 1010, antioxidant 1076, antioxidant 3114, antioxidant 168, antioxidant 618, antioxidant 626, antioxidant 1098, antioxidant 1330, antioxidant 3114, antioxidant 1790, antioxidant 1024, antioxidant P-EPQ, antioxidant 9228, antioxidant 641, antioxidant B215, antioxidant B225, and antioxidant B900.

[0018] The second aspect of the embodiment of the present application provides a method for preparing the modified polypropylene film as in the first aspect, comprising:

[0019] Weigh the raw materials according to weight;

[0020] The initiator and the silane compound are dissolved in acetone, and the dissolved solution is fully stirred and mixed with polypropylene, UV shielding nano powder and antioxidant in a high-speed mixer to obtain a mixture;

[0021] After the mixture is dried, it is melt-mixed by a twin-screw extruder, a sheet-like melt is extruded, and then a modified polypropylene film is obtained by a calender.

[0022] A second aspect of the embodiment of the present application provides a polypropylene-based photovoltaic backsheet, the polypropylene-based photovoltaic backsheet comprising:

[0023] An outer layer, the outer layer is made of the modified polypropylene film of the first aspect;

[0024] The inner layer is made of continuous fiber reinforced polypropylene composite material;

[0025] The outer layer and the inner layer are fused together by heat pressing.

[0026] In one embodiment, the continuous fiber reinforced polypropylene composite material is made of 2-6 layers of continuous fiber reinforced polypropylene prepreg tapes, which are laminated and hot-pressed and fused.

[0027] In one embodiment, the continuous fiber reinforced polypropylene prepreg tape comprises 20-60% polypropylene and 40-80% continuous fibers by weight.

[0028] In one embodiment, the continuous fiber is at least one of glass fiber, carbon fiber, aramid fiber, and basalt fiber.

[0029] The modified polypropylene film proposed in this application, on the one hand, benefits from the chemical shielding effect brought by the UV shielding functional group of the alkyl compound and the physical shielding effect brought by the UV physical shielding agent, which significantly enhances the film's tolerance to ultraviolet rays. On the other hand, the nano-powder physically reinforces the pure polypropylene substrate, which can effectively improve the film's mechanical properties such as stretching and tearing.

[0030] The continuous fiber reinforced polypropylene composite material in the polypropylene-based photovoltaic backplane proposed in this application combines the advantages of continuous fibers and thermoplastic polypropylene, and not only has ideal strength, modulus, and impact resistance, but is also environmentally friendly and recyclable. It is a preferred solution for replacing PET to make photovoltaic backplanes.

[0031] The polypropylene-based photovoltaic backplane proposed in this application uses environmentally friendly polypropylene as the polymer base material for both the inner and outer layers and is formed by hot pressing fusion, thereby eliminating the risk of aging and peeling of the traditional photovoltaic backplane adhesive layer from the source, ensuring the reliability and environmental protection of the photovoltaic backplane assembly during long-term use. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a schematic diagram of the structure of a polypropylene-based photovoltaic backsheet provided in an embodiment of the present application;

[0033] Figure 2 It is a reaction schematic diagram of the modified polypropylene film provided in the examples of the present application. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0035] It should be noted that although a logical order is shown in the flowchart, in some cases, the steps shown or described may be performed in a different order than that in the flowchart. The terms "first", "second", etc. in the specification, claims and the above drawings are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence.

[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein are only for the purpose of describing the embodiments of this application and are not intended to limit this application.

[0037] Based on the environmental and safety risks caused by fluorine in photovoltaic backsheets, the present invention provides a green fluorine-free polypropylene-based photovoltaic backsheet. The outer layer of the backsheet is made of a film made of modified polypropylene, and the inner layer is made of a continuous fiber reinforced polypropylene composite material. The two-layer structure is fused by hot pressing, eliminating the risk of aging of the bonding layer from the source, ensuring the reliability and environmental protection of the photovoltaic backsheet assembly in long-term use.

[0038] Reference Figure 1 , which shows a schematic structural diagram of a polypropylene-based photovoltaic backsheet provided in an embodiment of the present application.

[0039] like Figure 1 As shown, the polypropylene-based photovoltaic backsheet includes:

[0040] The outer layer is made of modified polypropylene film;

[0041] The inner layer is made of continuous fiber reinforced polypropylene composite material;

[0042] The outer layer and the inner layer are fused together by heat pressing.

[0043] The modified polypropylene film is made by a reaction extrusion process, and its thickness is 0.05-0.15 mm. The modified polypropylene film comprises the following components: polypropylene, initiator, silane compound, UV shielding nano powder, and antioxidant.

[0044] The components are in parts by weight, with polypropylene as the reference material, polypropylene is 100 parts, the initiator is 0.01-0.1 parts, the silane compound is 0.1-3 parts, the UV shielding nano powder is 5-50 parts, and the antioxidant is 1 part.

[0045] Wherein, the initiator is a peroxide initiator or an azo initiator. Exemplarily, the initiator is selected from at least one of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, cyclohexanone peroxide, di-tert-butyl peroxide, dibenzoyl peroxide (BPO), diisopropylbenzene peroxide, azobisisobutyronitrile, azobisisoheptylonitrile, and dimethyl azobisisobutyrate.

[0046] Wherein, the silane compound comprises a vinyl group, a UV shielding functional group and a hydrolysis functional group. Specifically, a free radical reaction is initiated by peroxide on polypropylene, and the silane compound is grafted, and the silane compound needs to simultaneously satisfy the vinyl group, UV shielding functional group and hydrolysis functional group required for grafting. Exemplarily, the silane compound is selected from at least one of vinyl triisopropenyloxysilane, vinyl triacetoxysilane, vinyl tributyl ketoxime silane, 3-methacryloxypropyl trimethoxysilane (G-570), 3-methacryloxypropyl triethoxysilane, 3-methacryloxypropyl tris (trimethylsiloxy) silane, 3-methacryloxypropyl methyl diethoxy silane, 3-methacryloxypropyl methyl dimethoxy silane, and tetramethyl tetraethylene cyclotetrasiloxane.

[0047] Wherein, the UV shielding nano powder is selected from at least one of nano titanium dioxide and nano zinc oxide.

[0048] Among them, the antioxidant is selected from at least one of antioxidant 1010, antioxidant 1076, antioxidant 3114, antioxidant 168, antioxidant 618, antioxidant 626, antioxidant 1098, antioxidant 1330, antioxidant 3114, antioxidant 1790, antioxidant 1024, antioxidant P-EPQ, antioxidant 9228, antioxidant 641, antioxidant B215, antioxidant B225, and antioxidant B900.

[0049] The method for preparing the modified polypropylene film comprises:

[0050] Weigh polypropylene, initiator, silane compound, UV shielding nano powder, and antioxidant according to weight proportions;

[0051] Dissolving the initiator and the silane compound with a small amount of acetone, and fully stirring and mixing the dissolved solution with polypropylene, UV shielding nano powder and antioxidant in a high-speed mixer to obtain a mixture;

[0052] After the mixture is dried, it is melt-mixed by a twin-screw extruder, a sheet-shaped melt is extruded, and then a modified polypropylene film is obtained by a calender. The twin-screw extruder adopts a co-rotating or counter-rotating twin-screw extruder, the cavity temperature is set at 100-220°C, and the screw speed is 10-100rpm.

[0053] The continuous fiber reinforced polypropylene composite material is obtained by hot pressing and fusing 2-6 layers of continuous fiber reinforced polypropylene prepreg tapes, wherein the interlayer cross angle can be set according to performance requirements, the hot pressing of the layers can be performed by a Teflon compounding machine, the hot pressing temperature is 180-250°C, and the thickness of the continuous fiber reinforced polypropylene composite material is 0.1-0.5mm. Exemplarily, 2 layers of continuous fiber reinforced polypropylene prepreg tapes can be hot pressed and fused at an angle of 0° / 90° or 0° / 45° to obtain a continuous fiber reinforced polypropylene composite material.

[0054] The continuous fiber reinforced polypropylene prepreg tape comprises 20-60% polypropylene and 40-80% continuous fiber in terms of mass percentage, wherein the continuous fiber is at least one of glass fiber, carbon fiber, aramid fiber and basalt fiber.

[0055] The modified polypropylene film and the continuous fiber reinforced polypropylene composite material are hot-pressed and fused by a Teflon compounding machine to form a polypropylene-based photovoltaic backplane at a hot-pressing temperature of 180-250°C.

[0056] The modified polypropylene film provided in the embodiment of the present application is prepared by a one-step reaction process, such as Figure 2 The example shown is a case of using dibenzoyl peroxide (BPO) as an initiator, 3-methacryloxypropyl trimethoxysilane (G-570) as a silane compound, and titanium dioxide as a physical shielding agent. The specific principle is: under heating conditions, the initiator decomposes into corresponding free radicals, which then capture hydrogen atoms in the main chain of polypropylene to form macromolecular free radicals, and the macromolecular free radicals and the vinyl double bonds of the silane compound undergo addition reactions, thereby completing the polypropylene-alkyl compound grafting reaction. Furthermore, the abundant hydroxyl groups on the surface of the nanoscale UV physical shielding agent react with the hydrolyzable functional groups of the alkyl compound under the action of adsorbed water, thereby constructing a covalent bond system that strongly links polypropylene-alkyl compound-UV physical shielding agent. The modified polypropylene film made therefrom, on the one hand, benefits from the chemical shielding effect brought by the UV shielding functional groups of the alkyl compound and the physical shielding effect brought by the UV physical shielding agent, significantly enhancing the film's tolerance to ultraviolet rays. On the other hand, the nanoscale powder physically reinforces the pure polypropylene substrate, which can effectively improve the film's mechanical properties such as tensile and tearing.

[0057] Continuous fiber reinforced polypropylene composite materials combine the advantages of continuous fiber and thermoplastic polypropylene. They not only have ideal strength, modulus, and impact resistance, but are also environmentally friendly and recyclable. They are the preferred option to replace PET for making photovoltaic backplanes.

[0058] The polypropylene-based photovoltaic backplane provided in the present application uses environmentally friendly polypropylene as the polymer base material for both the inner and outer layers and is formed by hot pressing fusion, thereby eliminating the risk of aging and peeling of the traditional photovoltaic backplane adhesive layer from the source, thereby ensuring the reliability and environmental protection of the photovoltaic backplane assembly during long-term use.

[0059] Example 1

[0060] The preparation method of polypropylene-based photovoltaic backsheet comprises the following steps:

[0061] (I) Preparation of the outer layer of the back sheet (modified polypropylene film):

[0062] S1: Weigh 0.01 parts of dibenzoyl peroxide BPO and 1.55 parts of vinyl triisopropyleneoxy silane, dissolve them in a small amount of acetone, and then stir and mix them with 100 parts of polypropylene, 27.5 parts of nano titanium dioxide and 1 part of antioxidant 1010 in a high-speed mixer.

[0063] S2: After drying, the product is fed into a twin-screw extruder to be melted and extruded into a sheet-like melt, and then subjected to a calender to obtain a 0.1 mm modified polypropylene film.

[0064] (ii) Preparation of backplane inner layer (continuous fiber reinforced polypropylene composite material):

[0065] Two layers of 0.2 mm glass fiber reinforced polypropylene prepreg tapes were selected and laid at an angle of 0° / 90°. The inner layer of the backplane was made by hot pressing, fusion and cooling in a Teflon compound machine.

[0066] (III) Preparation of photovoltaic backsheet:

[0067] The outer modified polypropylene film and the inner continuous fiber reinforced polypropylene composite material prepared in the first two steps are subjected to hot pressing, fusion and cooling by a Teflon compounding machine to obtain a photovoltaic backplane.

[0068] Example 2

[0069] The preparation method of polypropylene-based photovoltaic backsheet comprises the following steps:

[0070] (I) Preparation of back sheet outer layer (modified polypropylene film):

[0071] S1: Weigh 0.055 parts of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane and 3 parts of 3-methacryloxypropyltrimethoxysilane G-570, dissolve them in a small amount of acetone, and then stir and mix them with 100 parts of polypropylene, 5 parts of nano titanium dioxide and 1 part of antioxidant 1076 in a high-speed mixer.

[0072] S2: After drying, the product is fed into a twin-screw extruder to be melted and extruded into a sheet-like melt, and then subjected to a calender to obtain a 0.1 mm film.

[0073] (ii) Preparation of backplane inner layer (continuous fiber reinforced polypropylene composite material):

[0074] Two layers of 0.2 mm glass fiber reinforced polypropylene prepreg tapes were selected and laid at an angle of 0° / 45°. The inner layer of the backplane was made by hot pressing, fusion and cooling in a Teflon composite machine.

[0075] (III) Preparation of photovoltaic backsheet:

[0076] The outer modified polypropylene film and the inner continuous fiber reinforced polypropylene composite material prepared in the first two steps are subjected to hot pressing, fusion and cooling by a Teflon compounding machine to obtain a photovoltaic backplane.

[0077] Example 3

[0078] The preparation method of polypropylene-based photovoltaic backsheet comprises the following steps:

[0079] (I) Preparation of back sheet outer layer (modified polypropylene film):

[0080] S1: Weigh 0.1 parts of cyclohexanone peroxide and 0.1 parts of vinyl triacetoxysilane, dissolve them in a small amount of acetone, and fully stir and mix them with 100 parts of polypropylene, 50 parts of nano zinc oxide and 1 part of antioxidant 3114 in a high-speed mixer.

[0081] S2: After drying, the product is fed into a twin-screw extruder to be melted and extruded into a sheet-like melt, and then subjected to a calender to obtain a 0.1 mm film.

[0082] (ii) Preparation of backplane inner layer (continuous fiber reinforced polypropylene composite material):

[0083] Three layers of 0.2 mm glass fiber reinforced polypropylene prepreg tapes were selected and laid at an angle of 0° / 90° / 0°. The inner layer of the backplane was made by hot pressing, fusion and cooling in a Teflon composite machine.

[0084] (III) Preparation of photovoltaic backsheet:

[0085] The outer modified polypropylene film and the inner continuous fiber reinforced polypropylene composite material prepared in the first two steps are subjected to hot pressing, fusion and cooling by a Teflon compounding machine to obtain a photovoltaic backplane.

[0086] Example 4

[0087] The preparation method of polypropylene-based photovoltaic backsheet comprises the following steps:

[0088] (I) Preparation of back sheet outer layer (modified polypropylene film):

[0089] S1: Weigh 0.075 parts of di-tert-butyl peroxide and 1 part of vinyl trisbutyl ketoxime silane, dissolve them in a small amount of acetone, and then stir and mix them with 100 parts of polypropylene, 10 parts of nano titanium dioxide and 1 part of antioxidant 168 in a high-speed mixer.

[0090] S2: After drying, the product is fed into a twin-screw extruder to be melted and extruded into a sheet-like melt, and then subjected to a calender to obtain a 0.1 mm film.

[0091] (ii) Preparation of backplane inner layer (continuous fiber reinforced polypropylene composite material):

[0092] Three layers of 0.2 mm glass fiber reinforced polypropylene prepreg tapes were selected and laid at an angle of 0° / 45° / 0°. The inner layer of the backplane was made by hot pressing, fusion and cooling in a Teflon composite machine.

[0093] (III) Preparation of photovoltaic backsheet:

[0094] The outer modified polypropylene film and the inner continuous fiber reinforced polypropylene composite material prepared in the first two steps are subjected to hot pressing, fusion and cooling by a Teflon compounding machine to obtain a photovoltaic backplane.

[0095] Example 5

[0096] The preparation method of polypropylene-based photovoltaic backsheet comprises the following steps:

[0097] (I) Preparation of back sheet outer layer (modified polypropylene film):

[0098] S1: Weigh 0.025 parts of dicumyl peroxide and 2 parts of 3-methacryloxypropyl triethoxysilane, dissolve them in a small amount of acetone, and then stir and mix them with 100 parts of polypropylene, 40 parts of nano titanium dioxide and 1 part of antioxidant 1098 in a high-speed mixer.

[0099] S2: After drying, the product is fed into a twin-screw extruder to be melted and extruded into a sheet-like melt, and then subjected to a calender to obtain a 0.1 mm film.

[0100] (ii) Preparation of backplane inner layer (continuous fiber reinforced polypropylene composite material):

[0101] Four layers of 0.2 mm glass fiber reinforced polypropylene prepreg tapes were selected and laid at an angle of 0° / 90° / 0° / 90°. The inner layer of the backplane was made by hot pressing, fusion and cooling in a Teflon compound machine.

[0102] (III) Preparation of photovoltaic backsheet:

[0103] The outer modified polypropylene film and the inner continuous fiber reinforced polypropylene composite material prepared in the first two steps are subjected to hot pressing, fusion and cooling by a Teflon compounding machine to obtain a photovoltaic backplane.

[0104] Example 6

[0105] The preparation method of polypropylene-based photovoltaic backsheet comprises the following steps:

[0106] (I) Preparation of back sheet outer layer (modified polypropylene film):

[0107] S1: Weigh 0.03 parts of azobisisobutyronitrile and 2.5 parts of 3-methacryloxypropyltris(trimethylsiloxy)silane, dissolve them in a small amount of acetone, and then stir and mix them with 100 parts of polypropylene, 5 parts of nano titanium dioxide and 1 part of antioxidant 1330 in a high-speed mixer.

[0108] S2: After drying, the product is fed into a twin-screw extruder to be melted and extruded into a sheet-like melt, and then subjected to a calender to obtain a 0.1 mm film.

[0109] (ii) Preparation of backplane inner layer (continuous fiber reinforced polypropylene composite material):

[0110] Four layers of 0.2 mm glass fiber reinforced polypropylene prepreg tapes were selected and laid at an angle of 0° / 45° / 0° / 45°. The inner layer of the backplane was made by hot pressing, fusion and cooling in a Teflon composite machine.

[0111] (III) Preparation of photovoltaic backsheet:

[0112] The outer modified polypropylene film and the inner continuous fiber reinforced polypropylene composite material prepared in the first two steps are subjected to hot pressing, fusion and cooling by a Teflon compounding machine to obtain a photovoltaic backplane.

[0113] Example 7

[0114] The preparation method of polypropylene-based photovoltaic backsheet comprises the following steps:

[0115] (I) Preparation of back sheet outer layer (modified polypropylene film):

[0116] S1: Weigh 0.09 parts of azobisisoheptanenitrile and 0.5 parts of 3-methacryloxypropylmethyldiethoxysilane, dissolve them in a small amount of acetone, and stir and mix them with 100 parts of polypropylene, 50 parts of nano-titanium dioxide and 1 part of antioxidant P-EPQ in a high-speed mixer.

[0117] S2: After drying, the product is fed into a twin-screw extruder to be melted and extruded into a sheet-like melt, and then subjected to a calender to obtain a 0.1 mm film.

[0118] (ii) Preparation of backplane inner layer (continuous fiber reinforced polypropylene composite material):

[0119] Five layers of 0.2 mm glass fiber reinforced polypropylene prepreg tapes were selected and laid at an angle of 0° / 90° / 0° / 90° / 0°. The inner layer of the backplane was made by hot pressing, fusion and cooling in a Teflon compound machine.

[0120] (III) Preparation of photovoltaic backsheet:

[0121] The outer modified polypropylene film and the inner continuous fiber reinforced polypropylene composite material prepared in the first two steps are subjected to hot pressing, fusion and cooling by a Teflon compounding machine to obtain a photovoltaic backplane.

[0122] Example 8

[0123] The preparation method of polypropylene-based photovoltaic backsheet comprises the following steps:

[0124] (I) Preparation of back sheet outer layer (modified polypropylene film):

[0125] S1: Weigh 0.055 parts of dimethyl azobisisobutyrate and 1.55 parts of 3-methacryloxypropylmethyldimethoxysilane, dissolve them in a small amount of acetone, and stir and mix them with 100 parts of polypropylene, 27.5 parts of nano titanium dioxide and 1 part of antioxidant 9228 in a high-speed mixer.

[0126] S2: After drying, the product is fed into a twin-screw extruder to be melted and extruded into a sheet-like melt, and then subjected to a calender to obtain a 0.1 mm film.

[0127] (ii) Preparation of backplane inner layer (continuous fiber reinforced polypropylene composite material):

[0128] Six layers of 0.2 mm glass fiber reinforced polypropylene prepreg tapes were selected and laid at an angle of 0° / 45° / 0° / 45° / 0° / 45°. The inner layer of the backplane was made by hot pressing, fusion and cooling in a Teflon compound machine.

[0129] (III) Preparation of photovoltaic backsheet:

[0130] The outer modified polypropylene film and the inner continuous fiber reinforced polypropylene composite material prepared in the first two steps are subjected to hot pressing, fusion and cooling by a Teflon compounding machine to obtain a photovoltaic backplane.

[0131] Example 9

[0132] The preparation method of polypropylene-based photovoltaic backsheet comprises the following steps:

[0133] (I) Preparation of back sheet outer layer (modified polypropylene film):

[0134] S1: Weigh 0.055 parts of BPO and 1.55 parts of tetramethyltetravinylcyclotetrasiloxane, dissolve them in a small amount of acetone, and then stir and mix them with 100 parts of polypropylene, 27.5 parts of nano titanium dioxide and 1 part of antioxidant B225 in a high-speed mixer.

[0135] S2: After drying, the product is fed into a twin-screw extruder to be melted and extruded into a sheet-like melt, and then subjected to a calender to obtain a 0.1 mm film.

[0136] (ii) Preparation of backplane inner layer (continuous fiber reinforced polypropylene composite material):

[0137] Six layers of 0.2 mm glass fiber reinforced polypropylene prepreg tapes were selected and laid at an angle of 0° / 90° / 0° / 90° / 0° / 90°. The inner layer of the backplane was made by hot pressing, fusion and cooling in a Teflon composite machine.

[0138] (III) Preparation of photovoltaic backsheet:

[0139] The outer modified polypropylene film and the inner continuous fiber reinforced polypropylene composite material prepared in the first two steps are subjected to hot pressing, fusion and cooling by a Teflon compounding machine to obtain a photovoltaic backplane.

[0140] Comparative Example 1

[0141] The difference between Comparative Example 1 and Example 1 is that G-570 is not added in step S1.

[0142] Comparative Example 2

[0143] The difference between Comparative Example 2 and Example 1 is that nano titanium dioxide is not added in step S1.

[0144] Comparative Example 3

[0145] The difference between Comparative Example 3 and Example 1 is that G-570 and nano titanium dioxide are not added in step S1.

[0146] Comparative Example 4

[0147] The difference between Comparative Example 4 and Example 1 is that glass fiber is not added to the inner layer of the backboard for reinforcement.

[0148] The photovoltaic backsheets prepared in Examples 1-8 and Comparative Examples 1-4 were tested according to the photovoltaic module backsheet group standard T / CPIA0015-2019. The results are shown in the following table.

[0149] surface

[0150]

[0151] According to the above table, the photovoltaic backsheet provided by the embodiment of the present application has excellent UV resistance and yellowing resistance, which is due to the grafting of silane compounds containing UV absorbing functional groups on polypropylene under peroxide initiation, giving the matrix an intrinsic UV shielding function, and at the same time, the hydrolysis functional groups of the silane compounds are chemically coupled with the nanopowders with UV shielding function, so that the matrix can obtain mechanical reinforcement while further enhancing the UV shielding ability. In addition, the continuous glass fiber significantly improves the strength of the photovoltaic backsheet, and the thicker the continuous fiber reinforced polypropylene composite plate, the better the water vapor barrier performance.

[0152] The implementation methods described in the embodiments of the present application are intended to more clearly illustrate the technical solutions of the embodiments of the present application, and do not constitute a limitation on the technical solutions provided in the embodiments of the present application. Those skilled in the art will appreciate that with the evolution of technology and the emergence of new application scenarios, the technical solutions provided in the embodiments of the present application are also applicable to similar technical problems.

[0153] The various embodiments in the present application are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

[0154] It should also be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, commodity, or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, commodity, or apparatus.

[0155] The above are only embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.

Claims

1. A modified polypropylene film, characterized in that: The modified polypropylene film comprises the following components in parts by weight: Polypropylene 100 parts; Initiator 0.01-0.1 part; Silane compound 0.1-3 parts; 5-50 parts of UV shielding nano powder; 1 part antioxidant.

2. The modified polypropylene film according to claim 1, characterized in that: The initiator is a peroxide initiator or an azo initiator.

3. The modified polypropylene film according to claim 1, characterized in that: The silane compound comprises a vinyl group, a UV shielding functional group and a hydrolysis functional group.

4. The modified polypropylene film according to claim 1, characterized in that: The UV shielding nano powder is selected from at least one of nano titanium dioxide and nano zinc oxide.

5. The modified polypropylene film according to claim 1, characterized in that: The antioxidant is selected from at least one of antioxidant 1010, antioxidant 1076, antioxidant 3114, antioxidant 168, antioxidant 618, antioxidant 626, antioxidant 1098, antioxidant 1330, antioxidant 3114, antioxidant 1790, antioxidant 1024, antioxidant P-EPQ, antioxidant 9228, antioxidant 641, antioxidant B215, antioxidant B225, and antioxidant B900.

6. The method for preparing a modified polypropylene film according to claims 1 to 5, characterized in that: include: Weigh the raw materials according to weight; The initiator and the silane compound are dissolved in acetone, and the dissolved solution is fully stirred and mixed with polypropylene, UV shielding nano powder and antioxidant in a high-speed mixer to obtain a mixture; After the mixture is dried, it is melt-mixed by a twin-screw extruder, a sheet-shaped melt is extruded, and then the modified polypropylene film is obtained by a calender.

7. A polypropylene-based photovoltaic backsheet, characterized in that: The polypropylene-based photovoltaic backsheet comprises: An outer layer, wherein the outer layer is made of the modified polypropylene film as described in claims 1 to 5; An inner layer, wherein the inner layer is made of a continuous fiber reinforced polypropylene composite material; The outer layer and the inner layer are fused and formed by hot pressing.

8. The polypropylene-based photovoltaic backsheet according to claim 7, characterized in that: The continuous fiber reinforced polypropylene composite material is made of 2 to 6 layers of continuous fiber reinforced polypropylene prepreg tapes, which are laminated, hot-pressed and fused.

9. The polypropylene-based photovoltaic backsheet according to claim 8, characterized in that: The continuous fiber reinforced polypropylene prepreg tape comprises 20-60% polypropylene and 40-80% continuous fibers in terms of mass percentage.

10. The polypropylene-based photovoltaic backsheet according to claim 9, characterized in that: The continuous fiber is at least one of glass fiber, carbon fiber, aramid fiber and basalt fiber.

Citation Information

Cited By

  • Weather-resistant anti-aging polypropylene material and preparation method thereof

    CN120310136A