By growing the ε-Ga2O3 intrinsic layer on a 4H-SiC substrate and combining it with NiO film design, the problem of the difficulty of ε-Ga2O3 daily blind photodetector dissipating heat at high temperatures is solved, the usage and power consumption of Ga2O3 are reduced, and the use and power consumption of Ga2O3 are improved. The detection performance and stability achieve efficient photoelectric detection effect.

CN118983367AActive Publication Date: 2024-11-19SUN YAT SEN UNIV

Patent Information

Application Number
CN202411037412.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

ε-Ga2O3 daily blind photodetectors have problems of high energy consumption, low light-dark ratio and poor stability at high temperatures. They are mainly due to their low thermal conductivity, which leads to difficulty in dissipating heat. The prior art increases the thickness of the Ga2O3 layer to reduce dark current but leads to heating. Seriously, the cost has also increased significantly.

Method used

Using an ε-Ga2O3-based PIN structure heterojunction sun blind ultraviolet detector, the ε-Ga2O3 intrinsic layer was grown on a 4H-SiC substrate, and the high thermal conductivity of SiC was used to transfer heat, and the NiO film and round structure design was reduced. Photo loss and electrical resistance are prepared in combination with radio frequency magnetron sputtering and electron beam evaporation processes to form a PIN structure heterojunction.

Benefits of technology

Effectively reduces the usage of Ga2O3, reduces power consumption, improves detection performance and crystallization quality of the photodetector, maintains high light-dark ratio and stable time response characteristics, and maintains a high photocurrent even at 200℃. and low dark current.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983367A_ABST
    Figure CN118983367A_ABST
Patent Text Reader

Abstract

The invention discloses an epsilon-Ga2O3-based PIN structure heterojunction solar-blind ultraviolet detector and a preparation method thereof, and a detector prepared from a new material. The scheme is provided for solving the problems of high power consumption and the like in the prior art. Comprising a top electrode, a NiO thin film, an epsilon-Ga2O3 intrinsic layer, a 4H-SiC substrate and a bottom electrode which are sequentially stacked. The preparation method comprises the following steps: pretreating the 4H-SiC substrate; carrying out metal organic chemical vapor deposition on an epsilon-Ga2O3 intrinsic layer; carrying out radio frequency magnetron sputtering on a NiO film; and preparing a top electrode and a bottom electrode through electron beam evaporation. The method has the advantages that the consumption of Ga2O3 is reduced, and the power consumption can be reduced. Epsilon-Ga2O3 is grown on the 4H-SiC substrate, and a large amount of heat of an epsilon-Ga2O3 intrinsic layer can be transferred from the 4H-SiC substrate based on the excellent heat conductivity of 4.9 W / cm * K of SiC. Meanwhile, the in-plane lattice constant difference between the epsilon-Ga2O3 crystal of the orthogonal structure and 4H-SiC is small, the crystal quality of an epsilon-Ga2O3 intrinsic layer can be improved, and the detection performance of the photoelectric detector is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a detector made of new materials, and in particular to an ε-Ga2O3-based PIN structure heterojunction solar-blind ultraviolet detector and a preparation method thereof. Background Art

[0002] The bandgap width of Ga2O3 material is 4.4-5.3eV, and the wavelength range corresponding to its absorption band edge is 250-280Nm, which can cover most of the solar-blind ultraviolet region without the need for additional energy band modulation. It is one of the most ideal materials for preparing solar-blind photodetectors.

[0003] In order to meet the working requirements of extreme environments such as high temperature and high pressure, solar-blind photodetectors need to have good heat dissipation capabilities. However, due to the low thermal conductivity of the ε-Ga2O3 material itself (0.1-0.3W / cm·K), the heat dissipation problem is precisely the biggest challenge for ε-Ga2O3 photodetectors. Therefore, in practical applications, Ga2O3 solar-blind photodetectors will have problems such as high energy consumption, low light-to-dark ratio, and poor stability when working at high temperatures.

[0004] CN115642197A discloses a Ga2O3-based PIN structure heterojunction solar-blind ultraviolet detector and its preparation method. It unilaterally pursues smaller dark current and higher signal-to-noise ratio, and excessively thickens the light absorption layer, including the use of Ga2O3 in both the N-type layer and the intrinsic layer. This causes a very serious problem of heating and extremely high power consumption. Moreover, if the amount of Ga2O3 used is doubled, combined with the process cost and material cost, its overall preparation cost will increase by about 4 times, which is not suitable for large-scale commercial use. Summary of the invention

[0005] The object of the present invention is to provide an ε-Ga2O3-based PIN structure heterojunction solar-blind ultraviolet detector and a preparation method thereof, so as to solve the problems existing in the above-mentioned prior art.

[0006] The ε-Ga2O3-based PIN structure heterojunction solar-blind ultraviolet detector described in the present invention comprises a top electrode, a NiO film, an ε-Ga2O3 intrinsic layer, a 4H-SiC substrate and a bottom electrode stacked in sequence from top to bottom; wherein the NiO film serves as a P-type layer, the ε-Ga2O3 intrinsic layer serves as a light absorption layer, and the 4H-SiC substrate serves as an N-type layer, thereby forming a PIN structure heterojunction.

[0007] The NiO film is a truncated cone structure, and the top electrode is a circular ring structure; the outer edge of the top electrode is aligned with the outer edge of the NiO film in a vertical position.

[0008] The NiO film extends a supporting portion on one side; and the top electrode extends a soldering portion above the supporting portion.

[0009] The method for preparing an ε-Ga2O3-based PIN structure heterojunction solar-blind ultraviolet detector described in the present invention comprises the following steps:

[0010] S1. Pretreatment of 4H-SiC substrate;

[0011] S2. Preparing an ε-Ga2O3 intrinsic layer on one side of a 4H-SiC substrate using metal organic chemical vapor deposition;

[0012] S3. Preparation of NiO thin film on ε-Ga2O3 intrinsic layer by RF magnetron sputtering;

[0013] S4 uses electron beam evaporation process to prepare the top electrode on the NiO film and the bottom electrode on the other side of the 4H-SiC substrate.

[0014] In step S1, the selected 4H-SiC substrate has a microtube density of ≤0.5 cm -2 , resistivity range is 0.015~0.025Ω*cm, wafer direction is Offaxis:4.0°toward±0.5°; first soak in H2O2 / H2O / HCl=1:6:1 solution, then move to H2O2 / H2O / NH3·H2O=1:5:1 for soaking, and finally transfer to HF (5%) solution for soaking to remove surface contaminants; finally rinse with deionized water five times and dry.

[0015] In step S2, MOCVD two-step growth is adopted, triethylgallium is selected as gallium source, deionized water is used as oxygen source, and argon is used as carrier gas;

[0016] The first growth step: growing the nucleation layer at 560 °C, with a constant VI / III ratio of 69 and a growth time of 30 min;

[0017] The second growth step: epitaxial layer at 640°C, growth time is 120 min.

[0018] The sputtering power was set to 130 W, the gas pressure in the chamber was 5 mT, the oxygen-argon ratio was 1:1, the deposition rate was 0.5 Nm / min, and the sputtering time was 30 min.

[0019] The hole concentration of the NiO film is about 5.1×10 19 cm -3 , the hole mobility is about 0.1 cm 2 / (Vs).

[0020] In step S4, the electron beam voltage is controlled to be ≥9.7KeV, and the power setting ratio is controlled to be 15% to 20%; the deposition rate of Ti is The deposition rate of Au is The electrode was alloyed by rapid thermal annealing in a nitrogen atmosphere at a temperature of 470°C for 1 min. A bottom electrode was prepared under the 4H-SiC substrate.

[0021] In step S4, the electron beam voltage is controlled to be ≥9.7KeV, and the power setting ratio is controlled to be 15% to 20%; the deposition rate of Ni is The deposition rate of Au is A top electrode is prepared on top of the NiO film.

[0022] The ε-Ga2O3-based PIN structure heterojunction solar-blind ultraviolet detector and its preparation method described in the present invention have the advantages that the usage of Ga2O3 is reduced, which can reduce power consumption. ε-Ga2O3 is grown on a 4H-SiC substrate. Based on the excellent thermal conductivity of SiC of 4.9W / cm·K, a large amount of heat in the ε-Ga2O3 intrinsic layer can be transferred from the 4H-SiC substrate. At the same time, the difference in the in-plane lattice constant between the orthorhombic ε-Ga2O3 crystal and 4H-SiC is small, which can improve the crystallization quality of the ε-Ga2O3 intrinsic layer, thereby improving the detection performance of the photodetector. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a structural schematic diagram of the solar-blind ultraviolet detector described in the present invention.

[0024] Figure 2 It is a transmittance curve diagram of the P-NiO film described in the present invention.

[0025] Figure 3 It is an X-ray diffraction scan of the ε-Ga2O3 intrinsic layer described in the present invention.

[0026] Figure 4 It is an IV characteristic curve diagram of the solar-blind ultraviolet detector described in the present invention under different light intensities.

[0027] Figure 5 It is a light response IV curve diagram of the solar-blind ultraviolet detector described in the present invention at different temperatures, in the dark state and under 254Nm illumination.

[0028] Figure 6 It is the normalized IT characteristic curve of the solar-blind ultraviolet detector described in the present invention at 0V bias and different temperatures,

[0029] Figure 7 is the τ of the solar-blind ultraviolet detector described in the present invention at different temperatures d Summary diagram.

[0030] Reference numerals:

[0031] 10-top electrode, 11-weld metal part;

[0032] 20-NiO film, 21-supporting part;

[0033] 30-ε-Ga2O3 intrinsic layer;

[0034] 40-4H-SiC substrate;

[0035] 50 - bottom electrode. DETAILED DESCRIPTION

[0036] like Figure 1 As shown, the ε-Ga2O3-based PIN structure heterojunction day-blind ultraviolet detector described in the present invention includes a top electrode 10, a NiO film 20, an ε-Ga2O3 intrinsic layer 30, a 4H-SiC substrate 40 and a bottom electrode 50 stacked in sequence from top to bottom; wherein the NiO film 20 serves as a P-type layer, the ε-Ga2O3 intrinsic layer 30 serves as a light absorption layer, and the 4H-SiC substrate 40 serves as an N-type layer, thereby forming a PIN structure heterojunction.

[0037] The NiO film 20 is a truncated cone structure, and the top electrode 10 is a circular ring structure; the outer edge of the top electrode 10 is vertically aligned with the outer edge of the NiO film 20 .

[0038] The NiO film 20 extends a supporting portion 21 on one side; the top electrode 10 extends a soldering portion 11 above the supporting portion 21 .

[0039] The method for preparing an ε-Ga2O3-based PIN structure heterojunction solar-blind ultraviolet detector described in the present invention comprises the following steps:

[0040] S1. Pre-treating the 4H-SiC substrate 40;

[0041] S2. Preparing ε-Ga2O3 intrinsic layer 30 on one side of 4H-SiC substrate 40 by metal organic chemical vapor deposition;

[0042] S3. A NiO film 20 is prepared on the ε-Ga2O3 intrinsic layer 30 by radio frequency magnetron sputtering;

[0043] S4 uses an electron beam evaporation process to form a top electrode 10 on the NiO film 20 , and a bottom electrode 50 on the other side of the 4H—SiC substrate 40 .

[0044] In step S1, the selected 4H-SiC substrate 40 has a microtube density of ≤0.5 cm -2, resistivity range is 0.015~0.025Ω*cm, wafer direction is Offaxis:4.0°toward±0.5°; first soak in H2O2 / H2O / HCl=1:6:1 solution, then move to H2O2 / H2O / NH3·H2O=1:5:1 for soaking, and finally transfer to HF (5%) solution for soaking to remove surface contaminants; finally rinse with deionized water five times and dry.

[0045] In step S2, MOCVD two-step growth is adopted, triethylgallium is selected as gallium source, deionized water is used as oxygen source, and argon is used as carrier gas;

[0046] The first growth step: growing the nucleation layer at 560 °C, with a constant VI / III ratio of 69 and a growth time of 30 min;

[0047] The second growth step: epitaxial layer at 640°C, growth time is 120 min.

[0048] The sputtering power was set to 130 W, the gas pressure in the chamber was 5 mT, the oxygen-argon ratio was 1:1, the deposition rate was 0.5 Nm / min, and the sputtering time was 30 min.

[0049] The hole concentration of the NiO film 20 is about 5.1×10 19 cm -3 , the hole mobility is about 0.1 cm 2 / (Vs).

[0050] In step S4, the electron beam voltage is controlled to be ≥9.7KeV, and the power setting ratio is controlled to be 15% to 20%; the deposition rate of Ti is The deposition rate of Au is The electrode was alloyed by rapid thermal annealing in a nitrogen atmosphere, the annealing temperature was 470° C., and the annealing time was 1 min. The bottom electrode 50 was prepared under the 4H—SiC substrate 40 .

[0051] In step S4, the electron beam voltage is controlled to be ≥9.7KeV, and the power setting ratio is controlled to be 15% to 20%; the deposition rate of Ni is The deposition rate of Au is A top electrode 10 is prepared on the NiO film 20 .

[0052] Experimental test analysis:

[0053] like Figure 2As shown, the absorption edge of the NiO film 20 is between 310Nm and 340Nm, and at the same time, it can maintain a transmittance of about 50% in the wavelength range of day-blind light. Its truncated cone design can minimize the light loss before reaching the absorption layer, and can also play the role of a P-type layer. Even if part of the ε-Ga2O3 intrinsic layer 30 is covered by the NiO film 20, sufficient light signals can be obtained at a transmittance of nearly 50%. The circular ring design of the top electrode 10 can minimize light blocking and can effectively derive electrical signals. The provision of the soldering gold portion 11 can provide good wiring conditions.

[0054] The X-ray diffraction (XRD) 2θ-ω scanning results of the ε-Ga2O3 intrinsic layer 30 grown on the 4H-SiC substrate 40 show that Figure 3 As shown in FIG. 1 , the diffraction peaks at 38.90° and 59.80° correspond to the (004) and (006) planes of ε-Ga2O3, respectively. The diffraction peak with the highest intensity corresponds to the (004) plane of 4H-SiC, and no other diffraction peaks are observed. It can be seen that the Ga2O3 film grown on the 4H-SiC substrate 40 is a pure ε-phase.

[0055] The results of testing the device under different light intensities of 254Nm are as follows Figure 4 As shown, the optical power density range is 0.76mW / cm 2 ~2.92mW / cm 2 , the voltage test range is -10V~3V. Obviously, under different light intensities, the device always shows typical rectification characteristics in the entire voltage test range. Under 0V bias, the device dark current is 5.81×10 -11 Ampere, at an optical power density of 2.92mW / cm 2 Under the sunlight-blind light, the photocurrent is 2.11×10 -8 A, the light-to-dark current ratio reaches 1.6×10 2 .

[0056] Figure 5 The photocurrent and dark current of the solar-blind UV detector under 0V condition change with increasing temperature. It can be seen that the device can still maintain a high photocurrent and a small dark current as the temperature rises. Even when working at 200℃, the light-to-dark current ratio of the device can be close to 10 3 .

[0057] Figure 6 The time response characteristics of solar-blind UV detectors at different operating temperatures at 0V are demonstrated. Figure 7 is the time constant τ of the device at different temperatures d It can be seen that as the operating temperature increases, the device still maintains a stable time response characteristic. Calculate the τ when the device is working at 200℃d =117ms, compared with τ at room temperature d =88ms, the degradation degree is low.

[0058] For those skilled in the art, various other corresponding changes and deformations can be made according to the technical solutions and concepts described above, and all of these changes and deformations should fall within the protection scope of the claims of the present invention.

Claims

1. A type of ε-Ga 2 O 3 Based on PIN structure heterojunction solar-blind ultraviolet detector, It is characterized in that It comprises a top electrode (10), a NiO film (20), an ε-Ga 2 O 3 Intrinsic layer (30), 4H-SiC substrate (40) and bottom electrode (50); wherein the NiO film (20) is used as a P-type layer, ε-Ga 2 O 3 The intrinsic layer (30) serves as a light absorption layer, and the 4H-SiC substrate (40) serves as an N-type layer, thereby forming a PIN structure heterojunction.

2. The ε-Ga according to claim 1 2 O 3 Based on PIN structure heterojunction solar-blind ultraviolet detector, It is characterized in that The NiO film (20) is a truncated cone structure, and the top electrode (10) is a circular ring structure; the outer edge of the top electrode (10) is vertically aligned with the outer edge of the NiO film (20).

3. The ε-Ga according to claim 2 2 O 3 Based on PIN structure heterojunction solar-blind ultraviolet detector, It is characterized in that The NiO film (20) extends a supporting portion (21) on one side; and the top electrode (10) extends a soldering portion (11) above the supporting portion (21).

4. The ε-Ga according to any one of claims 1 to 3 2 O 3 Preparation method of PIN structure heterojunction solar-blind ultraviolet detector, It is characterized in that The following steps are involved: S1. Pretreating the 4H-SiC substrate (40); S2. Preparation of ε-Ga on one side of a 4H-SiC substrate (40) using metal organic chemical vapor deposition 2 O 3 Intrinsic layer (30); S3. Using RF magnetron sputtering to deposit ε-Ga 2 O 3 A NiO film (20) is prepared on the intrinsic layer (30); S4 uses an electron beam evaporation process to prepare a top electrode (10) on the NiO film (20), and prepares a bottom electrode (50) on the other side of the 4H-SiC substrate (40).

5. The preparation method according to claim 4, It is characterized in that In step S1, the selected 4H-SiC substrate (40) has a microtube density of ≤0.5 cm -2 , the resistivity range is 0.015~0.025Ω*cm, the wafer direction is Offaxis:4.0°toward±0.5°; first soak in H 2 O 2 / H 2 O / HCl=1:6:1 solution, and then move to H 2 O 2 / H 2 O / NH 3 ·H 2 O=1:5:1 for immersion, and finally transferred to HF (5%) solution for immersion to remove surface pollutants; finally rinsed with deionized water five times and dried.

6. The preparation method according to claim 4, It is characterized in that In step S2, MOCVD two-step growth is adopted, triethylgallium is selected as gallium source, deionized water is used as oxygen source, and argon is used as carrier gas; The first growth step: growing the nucleation layer at 560 °C, with a constant VI / III ratio of 69 and a growth time of 30 min; The second growth step: epitaxial layer at 640°C, growth time is 120 min.

7. The preparation method according to claim 4, It is characterized in that In step S3, the sputtering power is set to 130 W, the gas pressure in the chamber is 5 mT, the oxygen-argon ratio is 1:1, the deposition rate is 0.5 Nm / min, and the sputtering time is 30 minutes.

8. The preparation method according to claim 7, It is characterized in that The hole concentration of the NiO film (20) is about 5.1×10 19 cm -3 , the hole mobility is about 0.1 cm 2 / (Vs).

9. The preparation method according to claim 4, It is characterized in that In step S4, the electron beam voltage is controlled to be ≥9.7KeV, and the power setting ratio is controlled to be 15% to 20%; the deposition rate of Ti is The deposition rate of Au is The electrode is alloyed by rapid thermal annealing in a nitrogen atmosphere, the annealing temperature is 470° C., and the annealing time is 1 minute; a bottom electrode (50) is prepared under the 4H-SiC substrate (40).

10. The preparation method according to claim 4, It is characterized in that In step S4, the electron beam voltage is controlled to be ≥9.7KeV, and the power setting ratio is controlled to be 15% to 20%; the deposition rate of Ni is The deposition rate of Au is A top electrode (10) is prepared on the NiO film (20).

Citation Information

Patent Citations

  • Transparent Ga2O3 p-i-n heterostructure solar-blind ultraviolet light detector and preparation method thereof

    CN112103354A

  • Heterojunction solar-blind ultraviolet detector with Ga2O3-based PIN structure and preparation method of heterojunction solar-blind ultraviolet detector

    CN115642197A

  • KR20230104380A

Cited By

  • Visual fibrous solar blind photoelectric detector and preparation method and application thereof

    CN121888753A

  • Polarized light detector and preparation method thereof

    CN121908633A

  • Gallium oxide heterojunction DUV sensor and method for manufacturing the same

    JP2026109522A