Circuit board and electroplating method thereof

Through step-by-step pulse plating and hole filling processes, the deep plating ability and uniformity of laser blind holes, mechanical blind holes and through holes in the circuit board are solved, and the high-quality conduction and plating uniformity of the circuit board are achieved.

CN118984545APending Publication Date: 2024-11-19DELTON TECH (GUANGZHOU) INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411040099.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

When the existing electroplating method has both laser blind holes, mechanical blind holes and through holes in the circuit board, it is difficult to ensure the deep plating ability of laser blind holes and the electroplating uniformity of mechanical blind holes, resulting in the sealing of laser blind holes and The bottom coating of the mechanical blind hole hole is too thin, which affects the quality of the circuit board.

Method used

Using step-by-step electroplating method, the first, second and third pulse electroplating processes are used to deposit conductive layers on the inner wall surfaces of laser blind holes, mechanical blind holes and through holes, and combined with the hole filling process, the deep plating capacity of each hole is ensured. and plating uniformity.

Benefits of technology

The deep plating ability and electroplating uniformity of high thickness-diameter blind passes are achieved, ensuring the normal conduction of blind holes and through holes, and improving the quality of the circuit board.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984545A_ABST
    Figure CN118984545A_ABST
Patent Text Reader

Abstract

The invention discloses a circuit board and an electroplating method thereof, and the electroplating method comprises the steps: carrying out the drilling of a multilayer circuit board, and forming a laser blind hole, a mechanical blind hole, and a through hole; performing copper deposition on the laser blind hole, the mechanical blind hole and the through hole to form a first conduction layer in the laser blind hole, the mechanical blind hole and the through hole; a first pulse electroplating process is adopted, a second conduction layer is deposited on the surface of the inner wall of the laser blind hole, a third conduction layer is deposited on the surface of the inner wall of the mechanical blind hole, and a fourth conduction layer is deposited on the surface of the inner wall of the through hole; adopting a second pulse electroplating process to deposit and form a fifth conduction layer on the surface of the inner wall of the mechanical blind hole, and deposit and form a sixth conduction layer on the surface of the inner wall of the through hole; and depositing and forming a sixth conduction layer on the surface of the inner wall of the through hole by adopting a third pulse electroplating process. By means of the method, when the laser blind hole, the mechanical blind hole and the through hole exist at the same time, the deep plating capacity and the electroplating uniformity of the blind hole and the through hole with the high thickness-diameter ratio are achieved through the step-by-step electroplating method, and the quality of the circuit board is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of circuit boards, and in particular to a circuit board and an electroplating method thereof. Background Art

[0002] With the rapid development of the PCB industry, the PCB structure has also undergone tremendous changes. The increase in PCB thickness, the decrease in aperture, electroplating and the increase in thickness-to-diameter ratio have brought more difficulties to electroplating production. In order to solve the electroplating difficulties, today's electroplating methods have gradually shifted from DC electroplating to pulse electroplating to improve electroplating production capabilities.

[0003] The existing electroplating method for circuit boards is usually a pulse electroplating method for a hole in the circuit board, such as a through hole or a blind hole. However, when there are laser blind holes with a high aperture ratio, mechanical blind holes, and through holes with a high aspect ratio in the circuit board, the existing electroplating method is used to ensure the copper thickness and deep plating ability of the through hole. For laser blind holes and mechanical blind holes, the laser blind holes will be sealed, resulting in a "core wrapping" problem, and the bottom plating layer of the mechanical blind holes will be too thin, resulting in a "crab leg" problem, resulting in insufficient deep plating ability and uneven electroplating, thereby affecting the quality of the circuit board. Summary of the invention

[0004] The present invention provides a circuit board and an electroplating method thereof. When laser blind holes, mechanical blind holes and through holes exist at the same time, a step-by-step electroplating method is used to achieve deep plating capability and electroplating uniformity for integrated blind and through holes with a high aspect ratio, thereby ensuring that both the blind holes and through holes can be normally conductive, thereby improving the quality of the circuit board.

[0005] In a first aspect, the present invention provides a method for electroplating a circuit board, comprising:

[0006] Drill holes on multi-layer circuit boards to form laser blind vias, mechanical blind vias and through holes;

[0007] Plating copper on the laser blind vias, mechanical blind vias and through holes to form a first conductive layer in the laser blind vias, mechanical blind vias and through holes;

[0008] Using a first pulse electroplating process, a second conductive layer is deposited on the inner wall surface of the laser blind hole to form a second conductive layer, a third conductive layer is deposited on the inner wall surface of the mechanical blind hole to form a third conductive layer, and a fourth conductive layer is deposited on the inner wall surface of the through hole to form a fourth conductive layer;

[0009] Using a second pulse electroplating process, a fifth conductive layer is deposited on the inner wall surface of the mechanical blind hole to form a fifth conductive layer, and a sixth conductive layer is deposited on the inner wall surface of the through hole to form a sixth conductive layer;

[0010] The seventh conducting layer is deposited on the inner wall surface of the through hole by adopting the third pulse electroplating process.

[0011] Optionally, a first pulse electroplating process is used to deposit a second conductive layer on the inner wall surface of the laser blind hole, a third conductive layer on the inner wall surface of the mechanical blind hole, and a fourth conductive layer on the inner wall surface of the through hole, including:

[0012] A first pulse electroplating process is adopted, and according to the pulse electroplating conditions of a first preset mother waveform, a second conductive layer is deposited on the inner wall surface of the laser blind hole to form a second conductive layer, a third conductive layer is deposited on the inner wall surface of the mechanical blind hole to form a third conductive layer, and a fourth conductive layer is deposited on the inner wall surface of the through hole to form a fourth conductive layer; the first preset mother waveform includes at least one period of a first DC waveform and at least one period of a plurality of first sub-waveforms; the electroplating time of the first DC waveform is the same as the electroplating time of each first sub-waveform;

[0013] The fifth conductive layer is deposited on the inner wall surface of the mechanical blind hole by using the second pulse electroplating process, and the sixth conductive layer is deposited on the inner wall surface of the through hole, including:

[0014] A second pulse electroplating process is adopted, and according to the pulse electroplating conditions of the second preset mother waveform, a fifth conductive layer is deposited on the inner wall surface of the mechanical blind hole, and a sixth conductive layer is deposited on the inner wall surface of the through hole; the second preset mother waveform includes at least one period of a second DC waveform and at least one period of a plurality of second sub-waveforms; the electroplating time of the second DC waveform is the same as the electroplating time of each second sub-waveform;

[0015] The seventh conductive layer is deposited on the inner wall surface of the through hole by using the third pulse electroplating process, including:

[0016] A seventh conductive layer is deposited on the inner wall surface of the through hole by adopting a third pulse electroplating process according to the pulse electroplating conditions of a third preset mother waveform; the third preset mother waveform includes at least one period of a third DC waveform and at least one period of a plurality of third sub-waveforms; the electroplating time of the third DC waveform is the same as the electroplating time of each third sub-waveform;

[0017] The electroplating durations of the first DC waveform, the second DC waveform and the third DC waveform are different, and the waveforms of the first sub-waveform, the second sub-waveform and the third sub-waveform are different.

[0018] Optionally, the first sub-waveform includes a first forward pulse waveform and a first reverse pulse waveform;

[0019] In one cycle of each first sub-waveform, the preset time ratio of the first forward pulse waveform and the first reverse pulse waveform is equal;

[0020] Of two adjacent first sub-waveforms, a preset current ratio of the first forward pulse waveform to the first reverse pulse waveform of the latter is greater than or equal to a preset current ratio of the first forward pulse waveform to the first reverse pulse waveform of the former;

[0021] The second sub-waveform includes a second forward pulse waveform and a second reverse pulse waveform;

[0022] In one cycle of each second sub-waveform, the preset time ratio of the second forward pulse waveform and the second reverse pulse waveform is equal;

[0023] Of two adjacent second sub-waveforms, a preset current ratio between the second forward pulse waveform and the second reverse pulse waveform of the latter is less than or equal to a preset current ratio between the second forward pulse waveform and the second reverse pulse waveform of the former;

[0024] The third sub-waveform includes a third forward pulse waveform and a third reverse pulse waveform;

[0025] Within one cycle of each third sub-waveform, in two adjacent third sub-waveforms, the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the latter is less than or equal to the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the former, and the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of the latter is less than or equal to the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of the former.

[0026] Optionally, the first sub-waveform further includes a pause waveform, and the pause waveform is arranged after the first reverse pulse waveform;

[0027] During the pause waveform stage, consumption of copper ions produced by the electrolytic reaction in the electroplating solution is stopped, so that the copper ion concentration increases.

[0028] Optionally, the copper ion concentration is greater than or equal to 80 g / L.

[0029] Optionally, the first preset mother waveform includes at least a first electroplating time period, a second electroplating time period and a third electroplating time period. In the first electroplating time period, the first preset mother waveform includes at least two first sub-waveforms, and the first preset current ratio of the first forward pulse waveform and the first reverse pulse waveform of each first sub-waveform is equal; in the second electroplating time period, the first preset mother waveform includes at least two first sub-waveforms, and the second preset current ratio of the first forward pulse waveform and the first reverse pulse waveform of each first sub-waveform is equal; in the third electroplating time period, the first preset mother waveform includes at least two first sub-waveforms, and the third preset current ratio of the first forward pulse waveform and the first reverse pulse waveform of each first sub-waveform is equal;

[0030] The first preset current ratio, the second preset current ratio and the third preset current ratio increase in sequence;

[0031] The second preset mother waveform includes at least a fourth electroplating time period and a fifth electroplating time period. In the fourth electroplating time period, the second preset mother waveform includes at least two second sub-waveforms, and the fourth preset current ratio of the second forward pulse waveform and the second reverse pulse waveform of each second sub-waveform is equal; in the fifth electroplating time period, the second preset mother waveform includes at least two second sub-waveforms, and the fifth preset current ratio of the second forward pulse waveform and the second reverse pulse waveform of each second sub-waveform is equal;

[0032] The fourth preset current ratio is greater than the fifth preset current ratio;

[0033] The third preset mother waveform includes at least a sixth electroplating time period and a seventh electroplating time period. During the sixth electroplating time period, the third preset mother waveform includes at least two third sub-waveforms, and the first preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of each third sub-waveform is equal, and the sixth preset current ratio of the third forward pulse waveform and the third reverse pulse waveform is equal; during the seventh electroplating time period, the third preset mother waveform includes at least two third sub-waveforms, and the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of each third sub-waveform decreases successively, and the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of each third sub-waveform decreases successively.

[0034] Optionally, the preset time ratio of the first forward pulse waveform and the first reverse pulse waveform is A1:A2, the first preset current ratio is m1:n1, the second preset current ratio is m2:n2, and the third preset current ratio is m3:n3; the preset time ratio of the second forward pulse waveform and the second reverse pulse waveform is A3:A4, the fourth preset current ratio is m4:n4, and the fifth preset current ratio is m5:n5; the first preset time ratio is A5:A6; in the seventh electroplating time period, the third preset mother waveform includes three third sub-waveforms, and the preset times of the third forward pulse waveform and the third reverse pulse waveform of the first third sub-waveform are Assume that the time ratio is A7:A8, and the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform is m6:n6; the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the second third sub-waveform is (A7-k1):(A8-k2), and the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform is m7:n7; the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the third third sub-waveform is (A7-2*k1):(A8-2*k2), and the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform is m8:n8;

[0035] Among them, 100:5≤A1:A2≤120:6, 1:2.0≤m1:n1≤1:2.3, 1:2.4≤m2:n2≤1:2.6, 1:2.7≤m3:n3≤1:2.9, 180:9≤A3:A4≤200:10, 1:2.8≤m4:n4≤1:3.1, 1:2.4≤m5:n5≤1:2.6; 180:9≤A5:A6≤200:10, 100:5≤A7:A8≤120:6, k1:k2=(20:1)*i, i is a positive integer, 1:2.8≤m6:n6≤1:3.1, 1:2.4≤m7:n7≤1:2.8, 1:2.3≤m8:n8≤1:2.5.

[0036] Optionally, the electroplating time of the second preset mother waveform is equal to the electroplating time of the third preset mother waveform, and the electroplating time of the first preset mother waveform is greater than the electroplating time of the second preset mother waveform.

[0037] Optionally, after the first pulse electroplating process is used to deposit a second conductive layer on the inner wall surface of the laser blind hole, a third conductive layer is deposited on the inner wall surface of the mechanical blind hole, and a fourth conductive layer is deposited on the inner wall surface of the through hole, a second pulse electroplating process is used to deposit a fifth conductive layer on the inner wall surface of the mechanical blind hole, and before a sixth conductive layer is deposited on the inner wall surface of the through hole, the method further includes:

[0038] The laser blind vias are filled with hole filling technology to ensure the electroplating quality of the laser blind vias;

[0039] After the fifth conductive layer is deposited on the inner wall surface of the mechanical blind hole by the second pulse electroplating process and the sixth conductive layer is deposited on the inner wall surface of the through hole by the third pulse electroplating process and before the seventh conductive layer is deposited on the inner wall surface of the through hole by the third pulse electroplating process, the method further includes:

[0040] The mechanical blind vias are filled with a hole filling process to ensure the electroplating quality of the mechanical blind vias.

[0041] In a second aspect, the present invention provides a circuit board, which is prepared by the above-mentioned circuit board electroplating method.

[0042] The technical solution of the present invention forms laser blind holes, mechanical blind holes and through holes by drilling holes on a multi-layer circuit board; copper is deposited on the laser blind holes, mechanical blind holes and through holes to form a first conductive layer in the laser blind holes, mechanical blind holes and through holes; a first pulse electroplating process is used to deposit a second conductive layer on the inner wall surface of the laser blind holes, a third conductive layer on the inner wall surface of the mechanical blind holes, and a fourth conductive layer on the inner wall surface of the through holes; a second pulse electroplating process is used to deposit a fifth conductive layer on the inner wall surface of the mechanical blind holes, and a sixth conductive layer on the inner wall surface of the through holes; a third pulse electroplating process is used to deposit a seventh conductive layer on the inner wall surface of the through holes. Through the above method, when laser blind holes, mechanical blind holes and through holes exist at the same time, the step-by-step electroplating method is used to achieve the deep plating capability and electroplating uniformity of the high aspect ratio blind through hole, ensuring that both the blind holes and through holes can be normally conductive, thereby improving the quality of the circuit board.

[0043] It should be understood that the contents described in this section are not intended to identify the key or important features of the embodiments of the present invention, nor are they intended to limit the scope of the present invention. Other features of the present invention will become easily understood through the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0045] Figure 1 A flow chart of a circuit board electroplating method provided in Embodiment 1 of the present invention;

[0046] Figures 2 to 4 A schematic diagram of the electroplating effect of laser blind vias and mechanical blind vias with different aperture ratios after a first pulse electroplating process provided in Embodiment 1 of the present invention;

[0047] Figures 5 to 7 A schematic diagram of the electroplating effect of mechanical blind holes with different aperture ratios after a second pulse electroplating process provided in the first embodiment of the present invention;

[0048] Figures 8 to 10 A schematic diagram of the electroplating effect at different positions of a through hole after a second pulse electroplating process provided in the first embodiment of the present invention;

[0049] Figures 11 to 13 A schematic diagram of the electroplating effect at different positions of a through hole after a third pulse electroplating process provided in the first embodiment of the present invention;

[0050] Fig.14A flow chart of a circuit board electroplating method provided in Embodiment 2 of the present invention;

[0051] Fig.15 A flow chart of a method for electroplating a circuit board provided in Embodiment 3 of the present invention. DETAILED DESCRIPTION

[0052] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0053] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0054] Embodiment 1

[0055] Figure 1 A flow chart of a circuit board electroplating method provided in Embodiment 1 of the present invention, Figures 2 to 4 A schematic diagram of the electroplating effect of laser blind vias and mechanical blind vias with different aperture ratios after a first pulse electroplating process provided in Embodiment 1 of the present invention, Figures 5 to 7 A schematic diagram of the electroplating effect of mechanical blind holes with different aperture ratios after a second pulse electroplating process provided in Embodiment 1 of the present invention, Figures 8 to 10 A schematic diagram of the electroplating effect at different positions of a through hole after a second pulse electroplating process provided in the first embodiment of the present invention, Figures 11 to 13 Schematic diagram of the electroplating effect of different positions of a through hole after a third pulse electroplating process provided in Embodiment 1 of the present invention. This embodiment can be applied to the situation where there are laser blind vias, mechanical blind vias and through holes in a circuit board at the same time, and the laser blind vias, mechanical blind vias and through holes need to be electroplated step by step, such as Figures 1 to 13 As shown, the electroplating method includes:

[0056] S110. Drill holes on a multi-layer circuit board to form laser blind holes, mechanical blind holes and through holes.

[0057] Among them, Laser Via Hole, also known as micro via hole, refers to a blind hole formed by drilling a circuit board with a laser. Mechanical Via Hole refers to a blind hole formed by traditional mechanical drilling and other methods. Through Hole refers to a through hole that penetrates all layers of the circuit board to connect the top layer and the bottom layer.

[0058] Specifically, before electroplating, drilling can be performed on the multilayer circuit board according to the design information to form laser blind holes, mechanical blind holes and through holes on the multilayer circuit board. Among them, the formation method of the laser blind hole can include laser drilling, etc., the formation method of the mechanical blind hole can include mechanical drilling, etc., and the formation method of the through hole can include mechanical drilling, etc. In this embodiment, the aperture size of the laser blind hole can include 4mil and 5mil, etc., and the thickness of the insulating layer of the laser blind hole is 3.8mil, that is, the aperture ratio of the laser blind hole is 1.05 and 1.32, etc. The aperture size of the mechanical blind hole can include 10mil, 12mil and 14mil, etc., and the thickness of the insulating layer of the mechanical blind hole is 13.5mil, that is, the aperture ratio of the mechanical blind hole is 0.74, 0.89 and 1.04, etc., and both the laser blind hole and the mechanical blind hole are blind holes with high aperture ratios. The through holes may be densely arranged, that is, the distances between two adjacent through holes with an aperture of 0.2 mm are 0.45 pitch, 0.5 pitch, 0.55 pitch and 0.6 pitch respectively; the distances between two adjacent through holes with an aperture of 0.25 mm are 0.5 pitch, 0.55 pitch, 0.6 pitch and 0.65 pitch respectively; the distances between two adjacent through holes with an aperture of 0.3 mm are 0.55 pitch, 0.6 pitch, 0.65 pitch and 0.7 pitch respectively; the distance between two adjacent through holes with an aperture of 0.15 mm is 0.8 pitch; and the distance between two adjacent through holes with an aperture of 0.175 mm is 0.8 pitch.

[0059] S120, copper is deposited on the laser blind vias, the mechanical blind vias and the through holes to form a first conductive layer in the laser blind vias, the mechanical blind vias and the through holes.

[0060] Among them, copper plating is a conductive layer formed by chemical reaction deposition on the surface of the insulating layer of the laser blind vias, mechanical blind vias and the inner walls of the through holes of the circuit board, making the laser blind vias, mechanical blind vias and the inner walls of the through holes of the circuit board conductive, ensuring the normal conduction of electrical signals.

[0061] Specifically, after forming the laser blind vias, mechanical blind vias and through holes on the circuit board, copper deposition is performed on the laser blind vias, mechanical blind vias and through holes, so that the conductive layer can be quickly deposited on the inner walls of the laser blind vias, mechanical blind vias and through holes, thereby forming a uniform first conductive layer on the inner walls of the laser blind vias, mechanical blind vias and through holes. In this embodiment, the thickness of the first conductive layer may include 0.3um-0.5um, which may be determined according to actual conditions and is not specifically limited here.

[0062] S130, using a first pulse electroplating process, depositing a second conductive layer on the inner wall surface of the laser blind hole, depositing a third conductive layer on the inner wall surface of the mechanical blind hole, and depositing a fourth conductive layer on the inner wall surface of the through hole.

[0063] Among them, the pulse plating process is to control the time ratio and current ratio of the pulse waveform and other parameters so that the circuit board can be quickly deposited in the plating solution containing bipolar molecules, so as to form a conductive layer with a certain thickness on the inner wall surface of the blind hole and the through hole, so as to realize the conduction of the electrical signal. The pulse plating process is conducive to the rapid attachment of the conductive layer to the inner wall of the laser blind hole, the mechanical blind hole and the through hole, and can improve the structure of the conductive layer, which is conducive to the formation of a dense, bright and uniform conductive layer, improve the electroplating uniformity and deep plating ability of the conductive layer in the blind hole and the through hole, reduce the internal stress of the conductive layer, and improve the deep plating ability of the conductive layer. In this embodiment, the materials of the second conductive layer, the third conductive layer and the fourth conductive layer can include but are not limited to copper, the plating solution can include an acidic solution, and the material of the plating solution can include sulfuric acid or copper sulfate.

[0064] Specifically, when electroplating the formed laser blind holes, mechanical blind holes and through holes, step-by-step electroplating can be adopted, that is, the first pulse electroplating process is adopted, and under certain electroplating conditions, by controlling the time ratio and current ratio of the pulse waveform, as well as the copper ion concentration in the electroplating solution, the laser blind holes, mechanical blind holes and through holes are electroplated simultaneously, so that the bipolar molecules in the electroplating solution can be quickly deposited on the inner wall surface of the laser blind hole to form the second conductive layer, deposited on the inner wall surface of the mechanical blind hole to form the third conductive layer, and deposited on the inner wall surface of the through hole to form the fourth conductive layer. It should be noted that when setting the electroplating conditions, it is necessary to ensure that the electroplating conditions can meet the deep plating ability and electroplating uniformity of the laser blind hole, that is, the control of the copper ion concentration in the electroplating solution and the pulse waveform must meet the electroplating requirements of the laser blind hole, so that the laser blind hole can achieve the required deep plating ability and electroplating uniformity. However, this electroplating condition cannot meet the deep plating capacity of mechanical blind holes and through holes. It can only ensure uniform electroplating at the bottom of the mechanical blind holes and through holes without causing crab feet problems, so that different electroplating conditions can be used in the subsequent electroplating process to achieve deep plating capacity and electroplating uniformity for mechanical blind holes and through holes.

[0065] For example, Figure 2It shows the copper plating effect of the laser blind hole. It can be seen that the aperture of the laser blind hole is 4.27mil, and the copper plating thickness on both sides of the inner wall of the laser blind hole are 0.74mil and 0.79mil respectively, which reaches the deep plating capability of the laser blind hole, and the thickness difference on both sides is small, indicating that the electroplating uniformity is achieved on the inner wall of the laser blind hole. Figure 3 and Figure 4 The copper plating effect of mechanical blind holes with different apertures is shown. It can be seen that Figure 3 The aperture of the mechanical blind hole is 10.26mil, and the copper plating thickness on both sides of the inner wall of the laser blind hole is 0.78mil and 0.79mil respectively. The thickness difference on both sides is small, indicating that the electroplating on the inner wall of the mechanical blind hole is uniform and there is no crab foot problem. Figure 4 The aperture of the mechanical blind hole is 14.3 mil, and the copper plating thickness on both sides of the inner wall of the laser blind hole is 0.76 mil and 0.72 mil respectively. The thickness difference on both sides is small, indicating that the electroplating on the inner wall of the mechanical blind hole is uniform and there is no crab foot problem.

[0066] S140, using a second pulse electroplating process to deposit a fifth conductive layer on the inner wall surface of the mechanical blind hole, and to deposit a sixth conductive layer on the inner wall surface of the through hole.

[0067] The materials of the fifth conductive layer and the sixth conductive layer may include but are not limited to copper.

[0068] Specifically, after the electroplating of the laser blind hole reaches the predetermined requirements, the mechanical blind hole and the through hole need to be electroplated to meet the electroplating requirements of the mechanical blind hole and the through hole. Since the requirements for electroplating conditions of the mechanical blind hole and the through hole are different, when electroplating the mechanical blind hole and the through hole, it is possible to first ensure that the mechanical blind hole reaches its deep plating capacity and electroplating requirements, and then ensure that the through hole meets the electroplating requirements. In this embodiment, when electroplating the mechanical blind hole and the through hole, the second pulse electroplating process is adopted. Under certain electroplating conditions, by controlling the time ratio and current ratio of the pulse waveform, the bipolar molecules in the electroplating solution can be quickly deposited on the inner wall surface of the mechanical blind hole to form the fifth conductive layer, and deposited on the inner wall surface of the through hole to form the sixth conductive layer. At this time, the inner wall surface of the mechanical blind hole and the inner wall surface of the through hole both form two conductive layers.

[0069] It should be noted that when setting the electroplating conditions for the second pulse electroplating process, it is necessary to ensure that the electroplating conditions meet the deep plating capacity and electroplating uniformity of the mechanical blind holes, so that the mechanical blind holes meet the electroplating requirements. At the same time, the deep plating capacity of the through holes must be ensured. However, under the electroplating conditions, the through holes cannot meet their copper thickness requirements. Therefore, it can provide a basic guarantee for the third electroplating of the through holes.

[0070] Exemplary, Figures 5 to 7 The electroplating effects of three mechanical blind holes with different apertures are shown. Figure 5 The diameter of the medium mechanical blind hole is 14.07mil. Figure 6 The diameter of the medium mechanical blind hole is 12.51mil. Figure 7 The aperture of the mechanical blind hole is 10.53 mil. It can be seen that after two pulse electroplatings, the inner wall surfaces of the three apertures of the mechanical blind holes have achieved deep plating capability and electroplating uniformity while ensuring that there is no crab foot problem. Figures 8 to 10 The electroplating effects of different areas of the through-hole are shown. It can be seen that the electroplating effects of the through-hole mouth and the hole formed by the two-pulse electroplating process are relatively uniform, achieving the uniformity of electroplating of the through-hole.

[0071] S150, using a third pulse electroplating process to deposit a seventh conductive layer on the inner wall surface of the through hole.

[0072] The seventh conductive layer may include but is not limited to copper.

[0073] Specifically, after both the laser blind vias and the mechanical blind vias have reached the deep plating capacity, since the through holes are densely arranged, and this large-area dense hole arrangement will cause some through holes to fail to meet the copper thickness requirements during the electroplating process, the through holes need to be electroplated again, that is, using the third pulse electroplating process. Under certain electroplating conditions, by controlling the time ratio and current ratio of the pulse waveform, the bipolar molecules in the plating solution can be quickly deposited on the inner wall surface of the through hole to form the seventh conductive layer, thereby achieving the deep plating capacity and electroplating uniformity of the through holes.

[0074] For example, Figures 11 to 13 The electroplating effects of different areas of the through-hole are shown. It can be seen that the through-hole formed by the third pulse electroplating process meets the required copper thickness requirement, and the copper plating thickness at the hole mouth and in the hole formed by electroplating is relatively uniform, achieving the electroplating uniformity and deep plating capability of the through-hole.

[0075] The technical solution of the embodiment of the present invention forms laser blind holes, mechanical blind holes and through holes by drilling holes on a multi-layer circuit board; copper is deposited on the laser blind holes, mechanical blind holes and through holes to form a first conductive layer in the laser blind holes, mechanical blind holes and through holes; a first pulse electroplating process is used to deposit a second conductive layer on the inner wall surface of the laser blind holes, a third conductive layer on the inner wall surface of the mechanical blind holes, and a fourth conductive layer on the inner wall surface of the through holes; a second pulse electroplating process is used to deposit a fifth conductive layer on the inner wall surface of the mechanical blind holes, and a sixth conductive layer on the inner wall surface of the through holes; a third pulse electroplating process is used to deposit a seventh conductive layer on the inner wall surface of the through holes. Through the above method, when laser blind holes, mechanical blind holes and through holes exist at the same time, the step-by-step electroplating method is used to achieve the deep plating capability and electroplating uniformity of the high aspect ratio blind through hole, ensuring that both the blind holes and through holes can be normally conductive, thereby improving the quality of the circuit board.

[0076] Embodiment 2

[0077] Fig.14 A flowchart of a circuit board electroplating method provided in Embodiment 2 of the present invention. In this embodiment, the specific implementation method of S130, using the first pulse electroplating process to deposit a second conductive layer on the inner wall surface of the laser blind hole, deposit a third conductive layer on the inner wall surface of the mechanical blind hole, and deposit a fourth conductive layer on the inner wall surface of the through hole is refined as follows:

[0078] A first pulse electroplating process is adopted, and according to the pulse electroplating conditions of a first preset mother waveform, a second conductive layer is deposited on the inner wall surface of the laser blind hole to form a second conductive layer, a third conductive layer is deposited on the inner wall surface of the mechanical blind hole to form a third conductive layer, and a fourth conductive layer is deposited on the inner wall surface of the through hole to form a fourth conductive layer; the first preset mother waveform includes at least one period of a first DC waveform and at least one period of a plurality of first sub-waveforms; the electroplating time of the first DC waveform is the same as the electroplating time of each first sub-waveform;

[0079] For S140, the second pulse electroplating process is used to deposit the fifth conductive layer on the inner wall surface of the mechanical blind hole, and the sixth conductive layer is deposited on the inner wall surface of the through hole. The specific implementation method is as follows:

[0080] A second pulse electroplating process is adopted, and according to the pulse electroplating conditions of the second preset mother waveform, a fifth conductive layer is deposited on the inner wall surface of the mechanical blind hole, and a sixth conductive layer is deposited on the inner wall surface of the through hole; the second preset mother waveform includes at least one period of a second DC waveform and at least one period of a plurality of second sub-waveforms; the electroplating time of the second DC waveform is the same as the electroplating time of each second sub-waveform;

[0081] And for S150, the specific implementation method of using the third pulse electroplating process to deposit and form the seventh conductive layer on the inner wall surface of the through hole is refined as follows:

[0082] A third pulse plating process is adopted to deposit and form a seventh conductive layer on the inner wall surface of the through hole according to the pulse plating conditions of the third preset mother waveform; the third preset mother waveform includes at least one cycle of a third DC waveform and at least one cycle of multiple third sub-waveforms; the plating time of the third DC waveform is the same as the plating time of each third sub-waveform.

[0083] like Fig.14 As shown, the electroplating method includes:

[0084] S210, drilling holes on a multi-layer circuit board to form laser blind holes, mechanical blind holes and through holes.

[0085] S220, copper is deposited on the laser blind vias, the mechanical blind vias and the through holes to form a first conductive layer in the laser blind vias, the mechanical blind vias and the through holes.

[0086] S230, using the first pulse plating process, according to the pulse plating conditions of the first preset mother waveform, depositing a second conductive layer on the inner wall surface of the laser blind hole, depositing a third conductive layer on the inner wall surface of the mechanical blind hole, and depositing a fourth conductive layer on the inner wall surface of the through hole.

[0087] Specifically, when the first pulse electroplating process is used to deposit a second conductive layer on the inner wall surface of the laser blind hole, a third conductive layer on the inner wall surface of the mechanical blind hole, and a fourth conductive layer on the inner wall surface of the through hole, the pulse electroplating condition can be set to a first preset mother waveform, and electroplating is performed according to the first preset mother waveform. By setting the waveform shape of the first preset mother waveform, as well as the waveform time ratio and current ratio, uniform deposition can be achieved on the inner walls of the laser blind hole, the mechanical blind hole, and the through hole, so that the second conductive layer is deposited on the inner wall surface of the laser blind hole, the third conductive layer is deposited on the inner wall surface of the mechanical blind hole, and the fourth conductive layer is deposited on the inner wall surface of the through hole.

[0088] It should be noted that, in the present embodiment, the first preset mother waveform includes at least one cycle of the first DC waveform and at least one cycle of multiple first sub-waveforms, and the electroplating time of the first DC waveform is the same as the electroplating time of each first sub-waveform. That is to say, when the second conductive layer is deposited on the inner wall surface of the laser blind hole, the third conductive layer is deposited on the inner wall surface of the mechanical blind hole, and the fourth conductive layer is deposited on the inner wall surface of the through hole, it is necessary to continuously use the first DC waveform for electroplating within an electroplating time period until the preset electroplating time is reached, such as the preset electroplating time is 10 minutes. Similarly, when the first sub-waveform is used for electroplating, it is necessary to continuously use a pulse waveform of the first sub-waveform for repeated electroplating within an electroplating time period until the preset electroplating time is reached. After the preset electroplating time is reached, it is necessary to use a second first sub-waveform for pulse electroplating, and use the pulse waveform of the first sub-waveform for repeated electroplating within an electroplating time period until the first preset electroplating time is reached. When the electroplating of each first sub-waveform is completed, it indicates that the deep plating capacity has reached the electroplating requirements of the laser blind hole, and the mechanical blind hole has no crab leg problem, then the pulse electroplating of the first sub-waveform is stopped. In addition, since the electroplating solution of the pulse electroplating process is an acidic solution, after the laser blind hole, mechanical blind hole and through hole inner wall are deposited with copper once to form the first conductive layer, if the first sub-waveform is quickly turned on for pulse electroplating on the surface of the first conductive layer of the laser blind hole, mechanical blind hole and through hole inner wall, the first conductive layer formed after the copper deposition is oxidized in the acidic electroplating solution, affecting the normal transmission of electrical signals. To prevent the first conductive layer from being oxidized, a first DC waveform is also set when designing the first preset mother waveform, and the first DC waveform is located before the first sub-waveform. That is to say, before using the first sub-waveform to perform pulse electroplating on the surface of the first conductive layer of the inner wall of the laser blind hole, the mechanical blind hole and the through hole, it is necessary to use the first DC waveform to perform pulse electroplating on the surface of the first conductive layer of the inner wall of the laser blind hole, the mechanical blind hole and the through hole, so as to first form a protective layer on the surface of the first conductive layer to prevent the first conductive layer from being oxidized.

[0089] S240, using a second pulse electroplating process, according to the pulse electroplating conditions of a second preset mother waveform, depositing a fifth conductive layer on the inner wall surface of the mechanical blind hole, and depositing a sixth conductive layer on the inner wall surface of the through hole.

[0090] Specifically, when the second pulse electroplating process is used to deposit the fifth conductive layer and the sixth conductive layer on the inner wall surfaces of the mechanical blind hole and the through hole respectively, the pulse electroplating conditions can be set to the second preset mother waveform, and electroplating can be performed according to the second preset mother waveform. By setting the waveform shape of the second preset mother waveform, as well as the waveform time ratio and the current ratio, uniform deposition on the inner walls of the mechanical blind hole and the through hole can be achieved, so that the fifth conductive layer is deposited on the inner wall surface of the mechanical blind hole, and the sixth conductive layer is deposited on the inner wall surface of the through hole.

[0091] It should be noted that, in this embodiment, the second preset mother waveform includes at least one cycle of the second DC waveform and at least one cycle of multiple second sub-waveforms; the electroplating time of the second DC waveform is the same as the electroplating time of each second sub-waveform. That is to say, when the fifth conductive layer is deposited on the inner wall surface of the mechanical blind hole and the sixth conductive layer is deposited on the inner wall surface of the through hole, it is necessary to continuously use the second DC waveform for electroplating within an electroplating time period until the second preset electroplating time is reached, such as the second preset electroplating time is 7 minutes. Similarly, when the second sub-waveform is used for electroplating, it is necessary to continuously use a second sub-waveform pulse waveform for repeated electroplating within an electroplating time period until the second preset electroplating time is reached. After reaching the second preset electroplating time, it is necessary to use a second second sub-waveform for pulse electroplating, and repeat the second sub-waveform pulse waveform for repeated electroplating within an electroplating time period until the second preset electroplating time is reached. When the electroplating of each second sub-waveform is completed, it indicates that the deep plating ability has reached the electroplating requirements required by the mechanical blind hole, and the deep plating ability of the through hole is guaranteed at this time, then the second sub-waveform is stopped for pulse electroplating. In addition, in order to ensure that the second pulse plating process will not affect the conductive layer formed on the inner wall of the mechanical blind hole and the through hole when electroplating is performed, before using the second sub-waveform for electroplating, the second DC waveform will first be used to perform DC pulse plating on the surface of the third conductive layer on the inner wall of the mechanical blind hole and on the surface of the fourth conductive layer on the inner wall of the through hole, so that a protective layer can be formed on the surface of the third conductive layer and the surface of the fourth conductive layer to ensure the uniformity of the pulse plating.

[0092] S250, using a third pulse electroplating process, according to the pulse electroplating conditions of a third preset mother waveform, to deposit a seventh conductive layer on the inner wall surface of the through hole.

[0093] Specifically, when the third pulse plating process is used to deposit and form the seventh conductive layer on the inner wall surface of the through hole, the pulse plating conditions can be set to the third preset mother waveform, and electroplating can be performed according to the third preset mother waveform. By setting the waveform shape of the third preset mother waveform, as well as the waveform time ratio and current ratio, uniform deposition on the inner wall of the through hole can be achieved, so as to deposit and form the seventh conductive layer on the inner wall surface of the through hole.

[0094] It should be noted that, in this embodiment, the third preset mother waveform includes at least one cycle of the third DC waveform and at least one cycle of multiple third sub-waveforms; the electroplating time of the third DC waveform is the same as the electroplating time of each third sub-waveform. That is to say, when the seventh conductive layer is deposited on the inner wall surface of the through hole, it is necessary to continuously use the third DC waveform for electroplating within an electroplating time period until the third preset electroplating time is reached, such as the third preset electroplating time is 7 minutes. Similarly, when the third sub-waveform is used for electroplating, it is necessary to continuously use a pulse waveform of a third sub-waveform for repeated electroplating within an electroplating time period until the third preset electroplating time is reached. After reaching the third preset electroplating time, it is necessary to use a second third sub-waveform for pulse electroplating, and repeat the pulse waveform of the third sub-waveform for repeated electroplating within an electroplating time period until the second preset electroplating time is reached. When the electroplating of each third sub-waveform is completed, it indicates that the deep plating capacity has reached the electroplating requirements required for the through hole at this time, and then the third sub-waveform is stopped for pulse electroplating. In addition, in order to ensure that the third pulse plating process will not affect the conductive layer formed on the inner wall of the through hole, before using the third sub-waveform for electroplating, the third DC waveform will first be used to perform DC pulse plating on the surface of the sixth conductive layer on the inner wall of the through hole, so that a protective layer can be formed on the surface of the sixth conductive layer to ensure the uniformity of the pulse plating.

[0095] It is understandable that, since S230 to S250 represent the step-by-step electroplating method when blind through-holes exist at the same time, the electroplating duration of the first DC waveform in the first preset mother waveform, the second DC waveform in the second preset mother waveform, and the third DC waveform in the third preset mother waveform are different, and the waveforms of the first sub-waveform in the first preset mother waveform, the second sub-waveform in the second preset mother waveform, and the third sub-waveform in the third preset mother waveform are different. The specific configuration can be determined and set according to the actual situation, and is not limited here.

[0096] The technical solution of the embodiment of the present invention adopts the first pulse electroplating process, and according to the pulse electroplating conditions of the first preset mother waveform, the second conductive layer is deposited on the inner wall surface of the laser blind hole, the third conductive layer is deposited on the inner wall surface of the mechanical blind hole, and the fourth conductive layer is deposited on the inner wall surface of the through hole; the second pulse electroplating process is adopted, and according to the pulse electroplating conditions of the second preset mother waveform, the fifth conductive layer is deposited on the inner wall surface of the mechanical blind hole, and the sixth conductive layer is deposited on the inner wall surface of the through hole; the third pulse electroplating process is adopted, and according to the pulse electroplating conditions of the third preset mother waveform, the seventh conductive layer is deposited on the inner wall surface of the through hole. By using the above method, the deep plating ability and plating uniformity of the laser blind hole, mechanical blind hole and through hole are respectively achieved, and the quality and quality of the circuit board are improved.

[0097] In an optional embodiment, the first sub-waveform includes a first forward pulse waveform and a first reverse pulse waveform; within a cycle of each first sub-waveform, the preset time ratio of the first forward pulse waveform and the first reverse pulse waveform is equal; in two adjacent first sub-waveforms, the preset current ratio of the first forward pulse waveform and the first reverse pulse waveform of the latter is greater than or equal to the preset current ratio of the first forward pulse waveform and the first reverse pulse waveform of the former; the second sub-waveform includes a second forward pulse waveform and a second reverse pulse waveform; within a cycle of each second sub-waveform, the preset time ratio of the second forward pulse waveform and the second reverse pulse waveform is equal; in two adjacent second sub-waveforms, the latter The preset current ratio of the second forward pulse waveform and the second reverse pulse waveform of the latter is less than or equal to the preset current ratio of the second forward pulse waveform and the second reverse pulse waveform of the former; the third sub-waveform includes a third forward pulse waveform and a third reverse pulse waveform; within one cycle of each third sub-waveform, in two adjacent third sub-waveforms, the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the latter is less than or equal to the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the former, and the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of the latter is less than or equal to the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of the former.

[0098] Before introducing the structures of different preset mother waveforms, it is necessary to first briefly explain the principle of pulse electroplating. Generally, the pulse process used in pulse electroplating includes a forward pulse waveform and a reverse pulse waveform, that is, when the forward pulse waveform is used to electroplate the inner wall of the blind hole and the through hole, the bipolar molecules in the electroplating solution will carry a positive charge, and the cathode circuit board will carry a negative charge, so the positive charge will be close to the blind hole and the through hole of the cathode circuit board, thereby forming a stable diffusion layer on the inner wall of the blind hole and the through hole, so that the conductive layer can be evenly deposited on the inner wall surface of the blind hole and the through hole. After electroplating the inner wall of the blind hole and the through hole with a forward pulse waveform for a period of time, it will be converted to a reverse pulse waveform. During the reverse pulse waveform time, the inner wall of the blind hole and the through hole will not be pulse-plated, but a charge conversion will be performed, so that the negative charge of the cathode is converted to a positive charge, and the positive charge of the bipolar molecules is converted to a negative charge and thus close to the cathode. Since the orifice of the blind hole and the through hole is a high potential area, the bipolar molecules will quickly approach the cathode for deposition, which increases the thickness of the conductive layer at the orifice, forming a phenomenon of thick orifice and thin in the hole. When the reverse pulse waveform electroplating time ends, the pulse waveform will be changed back to a forward pulse waveform for electroplating. At this time, the cathode surface will be polarized to carry a negative charge, while the bipolar molecules at the orifice in the high potential area still retain a negative charge, so they will not continue to deposit at the orifice, thus forming an inhibition layer with a certain thickness to prevent the conductive layer from being deposited too thick at the orifice. The hole is a low potential area, which can maintain normal deposition of the conductive layer, thus achieving uniform electroplating on the inner wall of the blind hole and the through hole.

[0099] Based on the above pulse electroplating principle, in order to form a uniform conductive layer with a certain thickness on the inner wall surface of the laser blind hole, mechanical blind hole and through hole, and to prevent the phenomenon of too thick hole mouth and too thin hole, it is necessary to optimize the first sub-waveform, the second sub-waveform and the third sub-waveform. In this embodiment, the first sub-waveform includes a first forward pulse waveform and a first reverse pulse waveform; for each first sub-waveform, within a cycle of each first sub-waveform, the preset time ratio of the first forward pulse waveform and the first reverse pulse waveform is equal; in two adjacent first sub-waveforms, the preset current ratio of the first forward pulse waveform and the first reverse pulse waveform of the latter is greater than or equal to the preset current ratio of the first forward pulse waveform and the first reverse pulse waveform of the former. In other words, the cycle of a first preset mother waveform at least includes the sum of the electroplating time of each first sub-waveform. In this embodiment, the preset time ratio and the preset current ratio of the first forward pulse waveform and the first reverse pulse waveform in each first sub-waveform can be set. That is, the preset time ratios of the first forward pulse waveform and the first reverse pulse waveform in each first sub-waveform are set to be equal, and the preset time ratio may be 100:5. In two adjacent first sub-waveforms, the preset current ratio of the latter's first forward pulse waveform and the first reverse pulse waveform is set to be greater than or equal to the preset current ratio of the former's first forward pulse waveform and the first reverse pulse waveform, that is, the preset current ratio of the former's first forward pulse waveform and the first reverse pulse waveform may increase or remain unchanged compared with the preset current ratio of the latter's first forward pulse waveform and the first reverse pulse waveform, but for the first preset mother waveform, the preset current ratio of the latter's first forward pulse waveform and the first reverse pulse waveform is greater than the preset current ratio of the former's first forward pulse waveform and the first reverse pulse waveform, that is, the preset current ratio of the first forward pulse waveform and the first reverse pulse waveform is in an increasing form, so that the copper ions can be deposited normally when the preset current is relatively small, and the intensity of the laser blind hole pulse waveform is increased when the preset current ratio increases, so that the inner wall surface of the laser blind hole can be quickly deposited, so as to meet the copper thickness requirement of the laser blind hole, realize the deep plating ability and electroplating uniformity of the laser blind hole, and the mechanical blind hole has no crab feet problem.

[0100] Similarly, the second sub-waveform is set to include a second forward pulse waveform and a second reverse pulse waveform; for each second sub-waveform, within one cycle of each second sub-waveform, the preset time ratio of the second forward pulse waveform and the second reverse pulse waveform is equal, and the preset time ratio can be 200:10. In two adjacent second sub-waveforms, the preset current ratio of the second forward pulse waveform and the second reverse pulse waveform of the latter is less than or equal to the preset current ratio of the second forward pulse waveform and the second reverse pulse waveform of the former, that is, the preset current ratio of the second forward pulse waveform and the second reverse pulse waveform of the former may be reduced or unchanged compared with the preset current ratio of the second forward pulse waveform and the second reverse pulse waveform of the latter, but for the second preset mother waveform, the preset current ratio of the second forward pulse waveform and the second reverse pulse waveform of the latter second sub-waveform is less than the preset current ratio of the second forward pulse waveform and the second reverse pulse waveform of the former second sub-waveform, that is, the preset current ratio of the second forward pulse waveform and the second reverse pulse waveform of the second sub-waveform is in a decreasing form, so that the deep plating ability of the mechanical blind hole can be improved when the preset current is relatively large, so that the mechanical blind hole can meet the required copper thickness requirements. When the mechanical blind hole meets the electroplating requirements, the preset current ratio will be reduced to avoid excessive copper thickness on the inner wall of the mechanical blind hole, resulting in a "big belly" phenomenon with a thick hole bottom and a thin hole mouth, and the problem of rough inner wall surface of the mechanical blind hole, so as to ensure uniform electroplating and smooth surface on the basis of achieving the deep plating capability of the mechanical blind hole.

[0101] Similarly, the third sub-waveform is set to include a third forward pulse waveform and a third reverse pulse waveform; within one cycle of each third sub-waveform, in two adjacent third sub-waveforms, the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the latter is less than or equal to the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the former, and the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of the latter is less than or equal to the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of the former, that is, the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the former is less than or equal to the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of the former. The time ratio may decrease or remain unchanged compared with the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the latter, but for the third preset mother waveform, the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the latter's third sub-waveform is smaller than the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the former's third sub-waveform, that is, the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the third sub-waveform is in a decreasing form, so that the deep plating capability of the through hole can be achieved while avoiding the "big belly" phenomenon of thick hole and thin hole mouth, thereby ensuring uniform electroplating. In addition, in two adjacent third sub-waveforms, the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of the former may be reduced or unchanged compared with the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of the latter, but for the third preset mother waveform, the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of the latter third sub-waveform is less than the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of the former third sub-waveform, that is, the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of the third sub-waveform is in a decreasing form, so that the deep plating ability of the through hole can be improved when the preset current is relatively large, so that the through hole can meet the required copper thickness requirements. When the through hole meets the electroplating requirements, the preset current ratio is reduced to avoid excessive copper thickness on the inner wall surface of the through hole, resulting in the "big belly" phenomenon of thick hole and thin hole mouth, and the problem of rough surface of the inner wall of the through hole, so as to achieve electroplating uniformity and surface flatness on the basis of ensuring the deep plating ability of the through hole.

[0102] In another specific embodiment, optionally, the first preset mother waveform includes at least a first electroplating time period, a second electroplating time period and a third electroplating time period. In the first electroplating time period, the first preset mother waveform includes at least two first sub-waveforms, and the first preset current ratio of the first forward pulse waveform and the first reverse pulse waveform of each first sub-waveform is equal; in the second electroplating time period, the first preset mother waveform includes at least two first sub-waveforms, and the second preset current ratio of the first forward pulse waveform and the first reverse pulse waveform of each first sub-waveform is equal; in the third electroplating time period, the first preset mother waveform includes at least two first sub-waveforms, and the third preset current ratio of the first forward pulse waveform and the first reverse pulse waveform of each first sub-waveform is equal; the first preset current ratio, the second preset current ratio and the third preset current ratio increase successively; the second preset mother waveform includes at least a fourth electroplating time period and a fifth electroplating time period. In the fourth electroplating time period, the second preset mother waveform includes at least two second sub-waveforms, and the first forward pulse waveform and the first reverse pulse waveform of each first sub-waveform are equal. The fourth preset current ratio of the second forward pulse waveform and the second reverse pulse waveform of the waveform is equal; in the fifth electroplating time period, the second preset mother waveform includes at least two second sub-waveforms, and the fifth preset current ratio of the second forward pulse waveform and the second reverse pulse waveform of each second sub-waveform is equal; the fourth preset current ratio is greater than the fifth preset current ratio; the third preset mother waveform includes at least the sixth electroplating time period and the seventh electroplating time period, in the sixth electroplating time period, the third preset mother waveform includes at least two third sub-waveforms, the first preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of each third sub-waveform is equal, and the sixth preset current ratio of the third forward pulse waveform and the third reverse pulse waveform is equal; in the seventh electroplating time period, the third preset mother waveform includes at least two third sub-waveforms, the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of each third sub-waveform decreases successively, and the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of each third sub-waveform decreases successively.

[0103] Optionally, the first sub-waveform also includes a pause waveform, and the pause waveform is arranged after the first reverse pulse waveform; in the pause waveform stage, consumption of copper ions produced by the electrolytic reaction in the electroplating solution is stopped to increase the copper ion concentration.

[0104] Optionally, the copper ion concentration is greater than or equal to 80 g / L.

[0105] Optionally, the electroplating time of the second preset mother waveform is equal to the electroplating time of the third preset mother waveform, and the electroplating time of the first preset mother waveform is greater than the electroplating time of the second preset mother waveform.

[0106] The pause waveform is used to increase the copper ion concentration in the electroplating solution so that the copper ion concentration reaches the copper ion required for laser blind hole electroplating.

[0107] Specifically, in order to ensure that the laser blind hole meets the electroplating requirements and the mechanical blind hole and through hole have no crab foot problem, when designing the first preset mother waveform, the first preset mother waveform can be designed as multiple first sub-waveforms, and the first preset mother waveform includes at least the first electroplating time period, the second electroplating time period and the third electroplating time period, and each first sub-waveform also includes a pause waveform. In different electroplating time periods, by setting the number of first sub-waveforms, the preset time ratio and the preset current ratio of the first forward pulse waveform and the first reverse pulse waveform in the first sub-waveform, and the time of the pause waveform, the deep plating ability and electroplating uniformity of the laser blind hole can be achieved, while ensuring that the mechanical blind hole and through hole have no crab foot problem. In addition, by setting the relationship between the preset current ratios, that is, setting the first preset current ratio, the second preset current ratio and the third preset current ratio to increase in sequence, it is possible to ensure that copper ions can be deposited normally when the preset current ratio is relatively small, and increase the intensity of the laser blind hole pulse waveform when the preset current ratio increases, so that the inner wall surface of the laser blind hole can be quickly deposited, meeting the copper thickness requirements of the laser blind hole, realizing the deep plating ability and electroplating uniformity of the laser blind hole, and the mechanical blind hole has no crab feet problem.

[0108] It should be noted that, since the first preset current ratio, the second preset current ratio and the third preset current ratio increase in sequence, that is, the current of the reverse pulse waveform increases in sequence, more copper ions will be consumed, so that the copper ion concentration in the electroplating solution decreases rapidly. In order to ensure the electroplating effect and copper ion concentration requirements of the laser blind hole, the first sub-waveform is also provided with a pause waveform, so that the first sub-waveform pauses for a certain period of time. During the pause time, the copper ions generated by the electrolytic reaction in the electroplating solution are stopped from being consumed, so that the copper ion concentration increases and meets the copper ion requirements during the electroplating of the laser blind hole. In addition, according to the copper ion requirements of the laser blind hole, it is necessary to ensure that the copper ion concentration in the electroplating solution is greater than or equal to 80g / L. For example, the copper ion concentration can be 80g / L, 100g / L or 120g / L, which can be determined according to the actual situation and is not limited here.

[0109] Exemplarily, Table 1 is a schematic table of pulse parameters of a first preset mother waveform provided in Example 2 of the present invention. Referring to Table 1, the first preset mother waveform includes a first DC waveform and eight first sub-waveforms, the waveforms shown by reference numbers "1" to "8", wherein the electroplating time using the first preset mother waveform can be 90 minutes, and the current density is 14ASF. Under the electroplating conditions, the electroplating time using the first DC waveform and the electroplating time of each first sub-waveform are equal, that is, the electroplating time using the first DC waveform and the electroplating time of each first sub-waveform can be 10 minutes. During the electroplating time of 10 minutes, the blind holes and through holes in the circuit board are repeatedly electroplated with the pulse waveform until the plating time is reached, and then the next pulse waveform is used for repeated electroplating until the plating time is reached, and so on, until the electroplating is completed. In the first electroplating time period, the first preset mother waveform includes four first sub-waveforms, the pulse waveforms of the first first sub-waveform to the fourth first sub-waveform are the same, the preset time ratio of the first forward pulse waveform to the first reverse pulse waveform is 100:5, and the pause time is 6ms, that is, when the electroplating time of the first forward pulse waveform in each first sub-waveform is 100ms, the electroplating time of the first reverse pulse waveform is 5ms, and the electroplating time of a first sub-waveform is 111ms. The first preset current ratio of the first forward pulse waveform to the first reverse pulse waveform is 1:2.2, that is, when the current of the forward pulse waveform is 100A, the current of the corresponding reverse pulse waveform is -220A. In other words, first electroplating for 100ms with a forward pulse waveform with a current of 100A, then electroplating for 5ms with a reverse pulse waveform with a current of -220A, and finally pausing for 6ms, then a plating cycle of a first sub-waveform is completed. In the second electroplating time period, the first preset mother waveform includes two first sub-waveforms, the fifth first sub-waveform and the sixth first sub-waveform have the same pulse waveform, the preset time ratio of the first forward pulse waveform to the first reverse pulse waveform is 100:5, and the pause time is 6ms, that is, the electroplating time of a first sub-waveform is 111ms. The second preset current ratio of the first forward pulse waveform to the first reverse pulse waveform is 1:2.6, that is, when the current of the forward pulse waveform is 100A, the current of the corresponding reverse pulse waveform is -260A. In other words, first electroplating for 100ms with a forward pulse waveform with a current of 100A, then electroplating for 5ms with a reverse pulse waveform with a current of -260A, and finally pausing for 6ms, then a plating cycle of a first sub-waveform is completed. During the third electroplating time period, the first preset mother waveform includes two first sub-waveforms. The pulse waveforms of the seventh first sub-waveform and the eighth first sub-waveform are the same. The preset time ratio of the first forward pulse waveform to the first reverse pulse waveform is 100:5, and the pause time is 6ms, that is, the electroplating time of a first sub-waveform is 111ms.The third preset current ratio of the first forward pulse waveform to the first reverse pulse waveform is 1:2.8, that is, when the current of the forward pulse waveform is 100A, the current of the corresponding reverse pulse waveform is -280A. In other words, first electroplating with a forward pulse waveform with a current of 100A for 100ms, then electroplating with a reverse pulse waveform with a current of -280A for 5ms, and finally pausing for 6ms, then a plating cycle of a first sub-waveform is completed. It can be seen that the first preset current ratio, the second preset current ratio and the third preset current ratio increase in sequence.

[0110] Table 1 Schematic diagram of pulse parameters of the first preset mother waveform

[0111]

[0112] Similarly, when the laser blind hole meets the electroplating requirements and the deep plating ability of the mechanical blind hole is guaranteed, when designing the second preset mother waveform, the second preset mother waveform can be designed as a plurality of second sub-waveforms. The second preset mother waveform includes at least a fourth electroplating time period and a fifth electroplating time period. In different electroplating time periods, by setting the number of second sub-waveforms and the preset time ratio and preset current ratio of the second forward pulse waveform and the second reverse pulse waveform in each second sub-waveform, the deep plating ability and electroplating uniformity of the mechanical blind hole can be achieved. In addition, by setting the relationship between the preset current ratios, that is, setting the fourth preset current ratio to be greater than the fifth preset current ratio, the deep plating ability and electroplating requirements of the mechanical blind hole can be met, while avoiding the "big belly" phenomenon of the mechanical blind hole with a thick bottom and a thin hole mouth, thereby ensuring the electroplating quality of the mechanical blind hole.

[0113] Exemplarily, Table 2 is a schematic table of pulse parameters of a second preset mother waveform provided in Example 2 of the present invention. Referring to Table 2, the second preset mother waveform includes a second DC waveform and nine second sub-waveforms, the waveforms shown by reference numbers "1" to "9", wherein the electroplating time using the second preset mother waveform can be 75 minutes, and the current density is 15ASF. Under the electroplating conditions, the electroplating time using the second DC waveform is equal to the electroplating time of each second sub-waveform, that is, the electroplating time using the second DC waveform and the electroplating time of each second sub-waveform can be 7.5 minutes. During the electroplating time of 7.5 minutes, the blind holes and through holes in the circuit board are repeatedly electroplated with the pulse waveform until the plating time is reached, and then the next pulse waveform is used for repeated electroplating until the plating time is reached, and so on, until the electroplating is completed. In the fourth electroplating time period, the second preset mother waveform includes six second sub-waveforms, the pulse waveforms of the first second sub-waveform to the seventh second sub-waveform are the same, and the preset time ratio of the second forward pulse waveform to the second reverse pulse waveform is 200:10, that is, when the electroplating time of the second forward pulse waveform in each second sub-waveform is 200ms, the electroplating time of the second reverse pulse waveform is 10ms, and the electroplating time of a second sub-waveform is 210ms. The fourth preset current ratio of the second forward pulse waveform to the second reverse pulse waveform is 1:3, that is, when the current of the forward pulse waveform is 100A, the current of the corresponding reverse pulse waveform is -300A. In other words, first electroplating for 200ms with a forward pulse waveform with a current of 100A, and then electroplating for 10ms with a reverse pulse waveform with a current of -300A, two electroplating cycles of a second sub-waveform are completed. In the fifth electroplating time period, the second preset mother waveform includes two second sub-waveforms, the eighth second sub-waveform and the ninth second sub-waveform have the same pulse waveform, and the preset time ratio of the second forward pulse waveform to the second reverse pulse waveform is 200:10, that is, the electroplating time of a second sub-waveform is 210ms. The fifth preset current ratio of the second forward pulse waveform to the second reverse pulse waveform is 1:2.6, that is, when the current of the forward pulse waveform is 100A, the current of the corresponding reverse pulse waveform is -260A. In other words, first electroplating for 200ms with a forward pulse waveform with a current of 100A, and then electroplating for 10ms with a reverse pulse waveform with a current of -260A, two electroplating cycles of a second sub-waveform are completed. It can be seen that the fourth preset current ratio is greater than the fifth preset current ratio.

[0114] Table 2 Schematic diagram of pulse parameters of the second preset mother waveform

[0115]

[0116] Similarly, when the mechanical blind hole meets the electroplating requirements and needs to meet the copper thickness requirements of the through hole, when designing the third preset mother waveform, the third preset mother waveform can be designed as multiple third sub-waveforms. The third preset mother waveform includes at least the sixth electroplating time period and the seventh electroplating time period. In different electroplating time periods, by setting the number of third sub-waveforms and the preset time ratio and preset current ratio of the third forward pulse waveform and the third reverse pulse waveform in each third sub-waveform, the deep plating ability and electroplating uniformity of the through hole can be achieved. In addition, by setting the relationship between the preset current ratios and the relationship between the preset time ratios, that is, setting the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of each third sub-waveform to decrease in sequence, and the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of each third sub-waveform to decrease in sequence, so that the deep plating ability and electroplating requirements of the through hole can be met, while avoiding the "big belly" phenomenon of the through hole with a thick hole and a thin hole mouth, and the problem of rough surface of the inner wall of the through hole, the electroplating quality and surface flatness of the through hole can be ensured.

[0117] Exemplarily, Table 3 is a schematic table of pulse parameters of a third preset mother waveform provided in Example 2 of the present invention. Referring to Table 3, the third preset mother waveform includes a third DC waveform and nine third sub-waveforms, the waveforms shown by reference numbers "1" to "9", wherein the electroplating time using the third preset mother waveform can be 75 minutes. Under the electroplating conditions, the electroplating time using the third DC waveform and the electroplating time of each third sub-waveform are equal, that is, the electroplating time using the third DC waveform and the electroplating time of each third sub-waveform can both be 7.5 minutes. During the electroplating time of each 7.5 minutes, the through holes in the circuit board are repeatedly electroplated with the pulse waveform until the plating time is reached, and then the next pulse waveform is used for repeated electroplating until the plating time is reached, and so on, until the electroplating is completed. In the sixth electroplating time period, the third preset mother waveform includes six third sub-waveforms, the pulse waveforms of the first third sub-waveform to the sixth third sub-waveform are the same, and the preset time ratio of the third forward pulse waveform to the third reverse pulse waveform is 200:10, that is, when the electroplating time of the third forward pulse waveform in each third sub-waveform is 200ms, the electroplating time of the third reverse pulse waveform is 10ms, and the electroplating time of a third sub-waveform is 210ms. The fourth preset current ratio of the third forward pulse waveform to the third reverse pulse waveform is 1:3, that is, when the current of the forward pulse waveform is 100A, the current of the corresponding reverse pulse waveform is -300A. In other words, first electroplating for 200ms with a forward pulse waveform with a current of 100A, and then electroplating for 10ms with a reverse pulse waveform with a current of -300A, three electroplating cycles of a third sub-waveform are completed. In the seventh electroplating time period, the third preset mother waveform includes three third sub-waveforms, and the preset time ratio of the third forward pulse waveform to the third reverse pulse waveform of the seventh third sub-waveform is 100:5, and the preset current ratio is 1:3, that is, the preset time ratio is lower than the preset time ratio of the third forward pulse waveform to the third reverse pulse waveform in the first third sub-waveform to the sixth third sub-waveform. The preset time ratio of the third forward pulse waveform to the third reverse pulse waveform of the eighth third sub-waveform is 80:4, and the preset current ratio is 1:2.6, that is, the preset time ratio and the preset current ratio are both lower than the preset time ratio and the preset current ratio of the third forward pulse waveform to the third reverse pulse waveform in the first third sub-waveform to the sixth third sub-waveform. The preset time ratio of the third forward pulse waveform to the third reverse pulse waveform of the ninth third sub-waveform is 60:3, and the preset current ratio is 1:2.5, that is, the preset time ratio and the preset current ratio are lower than the preset time ratio and the preset current ratio of the third forward pulse waveform to the third reverse pulse waveform in the first third sub-waveform to the sixth third sub-waveform.It can be seen that the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of each third sub-waveform decreases successively, and the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of each third sub-waveform decreases successively, which can meet the deep plating capacity and electroplating requirements of the through hole while avoiding the "big belly" phenomenon of the through hole with a thick hole in the hole and a thin hole mouth, thereby ensuring the electroplating quality of the through hole.

[0118] Table 3 Schematic diagram of pulse parameters of the third preset mother waveform

[0119]

[0120]

[0121] Optionally, the preset time ratio of the first forward pulse waveform and the first reverse pulse waveform is A1:A2, the first preset current ratio is m1:n1, the second preset current ratio is m2:n2, and the third preset current ratio is m3:n3; the preset time ratio of the second forward pulse waveform and the second reverse pulse waveform is A3:A4, the fourth preset current ratio is m4:n4, and the fifth preset current ratio is m5:n5; the first preset time ratio is A5:A6; in the seventh electroplating time period, the third preset mother waveform includes three third sub-waveforms, and the preset times of the third forward pulse waveform and the third reverse pulse waveform of the first third sub-waveform are Assume that the time ratio is A7:A8, and the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform is m6:n6; the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the second third sub-waveform is (A7-k1):(A8-k2), and the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform is m7:n7; the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the third third sub-waveform is (A7-2*k1):(A8-2*k2), and the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform is m8:n8;

[0122] Among them, 100:5≤A1:A2≤120:6, 1:2.0≤m1:n1≤1:2.3, 1:2.4≤m2:n2≤1:2.6, 1:2.7≤m3:n3≤1:2.9, 180:9≤A3:A4≤200:10, 1:2.8≤m4:n4≤1:3.1, 1:2.4≤m5:n5≤1:2.6; 180:9≤A5:A6≤200:10, 100:5≤A7:A8≤120:6, k1:k2=(20:1)*i, i is a positive integer, 1:2.8≤m6:n6≤1:3.1, 1:2.4≤m7:n7≤1:2.8, 1:2.3≤m8:n8≤1:2.5.

[0123] Specifically, 100:5≤A1:A2≤120:6, that is, the ratio of A1:A2 is between 100:5 and 120:6, for example, A1:A2 can be 100:5 or 120:6, etc. The specific selection can be determined according to the design information of the laser blind hole of the circuit board, and no specific limitation is made here. 1:2.0≤m1:n1≤1:2.3, 1:2.4≤m2:n2≤1:2.6, 1:2.7≤m3:n3≤1:2.9, that is, the ratio of m1:n1 is between 1:2 and 1:2.3, the ratio of m2:n2 is between 1:2.4 and 1:2.6, and the ratio of m3:n3 is between 1:2.7 and 1:2.9. For example, m1:n1 can be 1:2, 1:2.1, 1:2.2 or 1:2.3, etc., m2:n2 can be 1:2.4, 1:2.5 or 1:2.6, etc., and m3:n3 can be 1:2.7, 1:2.8 or 1:2.9, etc. The specific selection can be determined according to the design information of the circuit board laser blind hole, and no specific limitation is made here. 180:9≤A3:A4≤200:10, that is, the ratio of A3:A4 is between 180:9 and 200:10, for example, A3:A4 can be 180:9 or 200:10, etc., and the specific selection can be determined according to the design information of the mechanical blind hole of the circuit board, and no specific limitation is made here. 1:2.8≤m4:n4≤1:3.1, 1:2.4≤m5:n5≤1:2.6; that is, the ratio of m4:n4 is between 1:2.8 and 1:3.1, and the ratio of m5:n5 is between 1:2.4 and 1:2.6, for example, m4:n4 can be 1:2.8, 1:2.9, 1:3 or 1:3.1, etc., and m2:n2 can be 1:2.4, 1:2.5 or 1:2.6, etc., and the specific selection can be determined according to the design information of the mechanical blind hole of the circuit board, and no specific limitation is made here. 180:9≤A5:A6≤200:10, 100:5≤A7:A8≤120:6, that is, the ratio of A5:A6 is between 180:9 and 200:10, and the ratio of A7:A8 is between 100:5 and 120:6, for example, A5:A6 can be 180:9 or 200:10, etc., and A7:A8 can be 100:5 or 120:6, etc. The specific selection can be determined according to the design information of the circuit board through hole, and no specific limitation is made here. Further, k1:k2=(20:1)*i, i is a positive integer, for example, k1:k2 can be 20:1, 40:1, 60:1 or 80:1, etc., which can be determined according to the design information, and no specific limitation is made here. 1:2.8≤m6:n6≤1:3.1, 1:2.4≤m7:n7≤1:2.8, 1:2.3≤m8:n8≤1:2.5.That is to say, the ratio of m6:n6 is between 1:2.8 and 1:3.1, the ratio of m7:n7 is between 1:2.4 and 1:2.8, and the ratio of m8:n8 is between 1:2.3 and 1:2.5. For example, m6:n6 can be 1:2.8, 1:2.9, 1:3 or 1:3.1, etc., m7:n7 can be 1:2.4, 1:2.5, 1:2.6, 1:2.7 or 1:2.8, etc., and m8:n8 can be 1:2.3, 1:2.4 or 1:2.5, etc. The specific selection can be determined based on the design information of the circuit board through-hole, and no specific limitation is made here.

[0124] Embodiment 3

[0125] Fig.15 A flowchart of a method for electroplating a circuit board provided in Embodiment 3 of the present invention, wherein after S130, using a first pulse electroplating process to deposit a second conductive layer on the inner wall surface of a laser blind hole, depositing a third conductive layer on the inner wall surface of a mechanical blind hole, and depositing a fourth conductive layer on the inner wall surface of a through hole, and S140, using a second pulse electroplating process to deposit a fifth conductive layer on the inner wall surface of a mechanical blind hole, and before depositing a sixth conductive layer on the inner wall surface of a through hole, the present embodiment further includes:

[0126] The laser blind vias are filled with hole filling technology to ensure the electroplating quality of the laser blind vias;

[0127] And after S140, using the second pulse electroplating process to deposit a fifth conductive layer on the inner wall surface of the mechanical blind hole and depositing a sixth conductive layer on the inner wall surface of the through hole, S150, using the third pulse electroplating process to deposit a seventh conductive layer on the inner wall surface of the through hole, the method further includes:

[0128] The mechanical blind vias are filled with a hole filling process to ensure the electroplating quality of the mechanical blind vias.

[0129] like Fig.15 As shown, the electroplating method includes:

[0130] S310, drilling holes on a multi-layer circuit board to form laser blind holes, mechanical blind holes and through holes.

[0131] S320, copper is deposited on the laser blind vias, the mechanical blind vias and the through holes to form a first conductive layer in the laser blind vias, the mechanical blind vias and the through holes.

[0132] S330, using a first pulse electroplating process, depositing a second conductive layer on the inner wall surface of the laser blind hole, depositing a third conductive layer on the inner wall surface of the mechanical blind hole, and depositing a fourth conductive layer on the inner wall surface of the through hole.

[0133] S340, fill the laser blind hole with a hole filling process to ensure the electroplating quality of the laser blind hole.

[0134] The hole filling process is to use conductive or non-conductive resin to fill holes such as laser through holes or mechanical blind buried vias by printing or other methods to achieve the purpose of plugging the holes. In this embodiment, the hole filling process may include a resin plugging process or the like.

[0135] Specifically, after the second conductive layer is deposited on the inner wall surface of the laser blind hole, the electroplating has reached the deep plating capacity and copper thickness requirements of the laser blind hole, that is, the electroplating of the laser blind hole is completed. In order to ensure that deposition will not continue in the laser blind hole during the subsequent electroplating process, affecting the electroplating effect of the laser blind hole, the laser blind hole can be filled, that is, the resin plugging process can be used to fill the laser blind hole, thereby ensuring the electroplating quality of the laser blind hole.

[0136] S350, using a second pulse electroplating process, depositing a fifth conductive layer on the inner wall surface of the mechanical blind hole, and depositing a sixth conductive layer on the inner wall surface of the through hole.

[0137] S360, use the hole filling process to fill the mechanical blind holes to ensure the electroplating quality of the mechanical blind holes.

[0138] Specifically, after the fifth conductive layer is deposited on the inner wall surface of the mechanical blind hole, the electroplating has reached the deep plating capacity and copper thickness requirements of the mechanical blind hole, that is, the electroplating of the mechanical blind hole is completed. In order to ensure that deposition will not continue in the mechanical blind hole during the subsequent electroplating process, affecting the electroplating effect of the mechanical blind hole, the mechanical blind hole can be filled, that is, the resin plug process can be used to fill the mechanical blind hole, thereby ensuring the electroplating quality of the mechanical blind hole.

[0139] S370, using a third pulse electroplating process to deposit a seventh conductive layer on the inner wall surface of the through hole.

[0140] The technical solution of the embodiment of the present invention adopts the first pulse electroplating process to deposit the second conductive layer on the inner wall surface of the laser blind hole, the third conductive layer on the inner wall surface of the mechanical blind hole, and the fourth conductive layer on the inner wall surface of the through hole; the laser blind hole is filled with a hole filling process to ensure the electroplating quality of the laser blind hole; the second pulse electroplating process is adopted to deposit the fifth conductive layer on the inner wall surface of the mechanical blind hole, and the sixth conductive layer on the inner wall surface of the through hole; the mechanical blind hole is filled with a hole filling process to ensure the electroplating quality of the mechanical blind hole; the third pulse electroplating process is adopted to deposit the seventh conductive layer on the inner wall surface of the through hole. The above method ensures the electroplating uniformity of the laser blind hole and the mechanical blind hole, avoids the influence on the subsequent electroplating of the through hole, and improves the quality of the circuit board.

[0141] Embodiment 4

[0142] Embodiment 4 of the present invention provides a circuit board, which is prepared by the above-mentioned circuit board electroplating method and has functional modules and beneficial effects corresponding to the execution method.

[0143] It should be understood that the various forms of processes shown above can be used to reorder, add or delete steps. For example, the steps described in the present invention can be executed in parallel, sequentially or in different orders, as long as the desired results of the technical solution of the present invention can be achieved, and this document does not limit this.

[0144] The above specific implementations do not constitute a limitation on the protection scope of the present invention. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions can be made according to design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for electroplating a circuit board, characterized in that: include: Drill holes on multi-layer circuit boards to form laser blind vias, mechanical blind vias and through holes; Performing copper deposition on the laser blind via, the mechanical blind via and the through hole to form a first conductive layer in the laser blind via, the mechanical blind via and the through hole; Using a first pulse electroplating process, a second conductive layer is deposited on the inner wall surface of the laser blind hole to form a second conductive layer, a third conductive layer is deposited on the inner wall surface of the mechanical blind hole to form a third conductive layer, and a fourth conductive layer is deposited on the inner wall surface of the through hole to form a fourth conductive layer; Using a second pulse electroplating process, a fifth conductive layer is deposited on the inner wall surface of the mechanical blind hole, and a sixth conductive layer is deposited on the inner wall surface of the through hole; A third pulse electroplating process is adopted to deposit and form a seventh conductive layer on the inner wall surface of the through hole.

2. The electroplating method according to claim 1, characterized in that: Using a first pulse electroplating process, depositing a second conductive layer on the inner wall surface of the laser blind hole, depositing a third conductive layer on the inner wall surface of the mechanical blind hole, and depositing a fourth conductive layer on the inner wall surface of the through hole, including: A first pulse electroplating process is adopted, and according to the pulse electroplating conditions of a first preset mother waveform, a second conductive layer is deposited on the inner wall surface of the laser blind hole, a third conductive layer is deposited on the inner wall surface of the mechanical blind hole, and a fourth conductive layer is deposited on the inner wall surface of the through hole; the first preset mother waveform includes at least one period of a first DC waveform and at least one period of a plurality of first sub-waveforms; the electroplating time of the first DC waveform is the same as the electroplating time of each of the first sub-waveforms; Using a second pulse electroplating process, depositing a fifth conductive layer on the inner wall surface of the mechanical blind hole, and depositing a sixth conductive layer on the inner wall surface of the through hole, including: A second pulse electroplating process is adopted, and according to the pulse electroplating conditions of a second preset mother waveform, a fifth conductive layer is deposited on the inner wall surface of the mechanical blind hole, and a sixth conductive layer is deposited on the inner wall surface of the through hole; the second preset mother waveform includes at least one period of a second DC waveform and at least one period of a plurality of second sub-waveforms; the electroplating time of the second DC waveform is the same as the electroplating time of each of the second sub-waveforms; The seventh conductive layer is deposited on the inner wall surface of the through hole by using a third pulse electroplating process, comprising: A seventh conductive layer is deposited on the inner wall surface of the through hole by adopting a third pulse electroplating process according to the pulse electroplating conditions of a third preset mother waveform; the third preset mother waveform includes at least one period of a third DC waveform and at least one period of a plurality of third sub-waveforms; the electroplating time of the third DC waveform is the same as the electroplating time of each of the third sub-waveforms; The electroplating durations of the first DC waveform, the second DC waveform, and the third DC waveform are different, and the waveforms of the first sub-waveform, the second sub-waveform, and the third sub-waveform are different.

3. The electroplating method according to claim 2, characterized in that: The first sub-waveform includes a first forward pulse waveform and a first reverse pulse waveform; In one cycle of each of the first sub-waveforms, the preset time ratios of the first forward pulse waveform and the first reverse pulse waveform are equal; Of two adjacent first sub-waveforms, a preset current ratio between the first forward pulse waveform and the first reverse pulse waveform of the latter is greater than or equal to a preset current ratio between the first forward pulse waveform and the first reverse pulse waveform of the former; The second sub-waveform includes a second forward pulse waveform and a second reverse pulse waveform; In one cycle of each of the second sub-waveforms, the preset time ratios of the second forward pulse waveform and the second reverse pulse waveform are equal; In two adjacent second sub-waveforms, a preset current ratio between the second forward pulse waveform and the second reverse pulse waveform of the latter is less than or equal to a preset current ratio between the second forward pulse waveform and the second reverse pulse waveform of the former; The third sub-waveform includes a third forward pulse waveform and a third reverse pulse waveform; Within one cycle of each of the third sub-waveforms, in two adjacent third sub-waveforms, the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the latter is less than or equal to the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the former, and the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of the latter is less than or equal to the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of the former.

4. The electroplating method according to claim 3, characterized in that: The first sub-waveform further includes a pause waveform, and the pause waveform is arranged after the first reverse pulse waveform; In the pause waveform stage, consumption of copper ions produced by electrolytic reaction in the electroplating solution is stopped, so that the copper ion concentration increases.

5. The electroplating method according to claim 4, characterized in that: The copper ion concentration is greater than or equal to 80 g / L.

6. The electroplating method according to claim 3, characterized in that: The first preset mother waveform at least includes a first electroplating time period, a second electroplating time period and a third electroplating time period. In the first electroplating time period, the first preset mother waveform includes at least two of the first sub-waveforms, and the first preset current ratio of the first forward pulse waveform to the first reverse pulse waveform of each of the first sub-waveforms is equal; in the second electroplating time period, the first preset mother waveform includes at least two of the first sub-waveforms, and the second preset current ratio of the first forward pulse waveform to the first reverse pulse waveform of each of the first sub-waveforms is equal; in the third electroplating time period, the first preset mother waveform includes at least two of the first sub-waveforms, and the third preset current ratio of the first forward pulse waveform to the first reverse pulse waveform of each of the first sub-waveforms is equal; The first preset current ratio, the second preset current ratio and the third preset current ratio are increased in sequence; The second preset mother waveform includes at least a fourth electroplating time period and a fifth electroplating time period. In the fourth electroplating time period, the second preset mother waveform includes at least two second sub-waveforms, and the fourth preset current ratio of the second forward pulse waveform to the second reverse pulse waveform of each second sub-waveform is equal; in the fifth electroplating time period, the second preset mother waveform includes at least two second sub-waveforms, and the fifth preset current ratio of the second forward pulse waveform to the second reverse pulse waveform of each second sub-waveform is equal; The fourth preset current ratio is greater than the fifth preset current ratio; The third preset mother waveform at least includes a sixth electroplating time period and a seventh electroplating time period. Within the sixth electroplating time period, the third preset mother waveform includes at least two third sub-waveforms, and the first preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of each of the third sub-waveforms is equal, and the sixth preset current ratio of the third forward pulse waveform and the third reverse pulse waveform is equal; within the seventh electroplating time period, the third preset mother waveform includes at least two third sub-waveforms, and the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of each of the third sub-waveforms decreases successively, and the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform of each of the third sub-waveforms decreases successively.

7. The electroplating method according to claim 6, characterized in that: The preset time ratio of the first forward pulse waveform and the first reverse pulse waveform is A1:A2, the first preset current ratio is m1:n1, the second preset current ratio is m2:n2, and the third preset current ratio is m3:n3; the preset time ratio of the second forward pulse waveform and the second reverse pulse waveform is A3:A4, the fourth preset current ratio is m4:n4, and the fifth preset current ratio is m5:n5; the first preset time ratio is A5:A6; in the seventh electroplating time period, the third preset mother waveform includes three third sub-waveforms, the preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the first third sub-waveform is A7:A8, and the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform is m6:n6; The preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the second third sub-waveform is (A7-k1): (A8-k2), and the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform is m7: n7. The preset time ratio of the third forward pulse waveform and the third reverse pulse waveform of the third third sub-waveform is (A7-2*k1): (A8-2*k2), and the preset current ratio of the third forward pulse waveform and the third reverse pulse waveform is m8: n8. Among them, 100:5≤A1:A2≤120:6, 1:2.0≤m1:n1≤1:2.3, 1:2.4≤m2:n2≤1:2.6, 1:2.7≤m3:n3≤1:2.9, 180:9≤A3:A4≤200:10, 1:2.8≤m4:n4≤1:3.1, 1:2.4≤m5:n5≤1:2.6; 180:9≤A5:A6≤200:10, 100:5≤A7:A8≤120:6, k1:k2=(20:1)*i, i is a positive integer, 1:2.8≤m6:n6≤1:3.1, 1:2.4≤m7:n7≤1:2.8, 1:2.3≤m8:n8≤1:2.

5.

8. The electroplating method according to claim 2, characterized in that: The electroplating time of the second preset mother waveform is equal to the electroplating time of the third preset mother waveform, and the electroplating time of the first preset mother waveform is greater than the electroplating time of the second preset mother waveform.

9. The electroplating method according to claim 1, characterized in that: After the first pulse electroplating process is used to deposit a second conductive layer on the inner wall surface of the laser blind hole, a third conductive layer is deposited on the inner wall surface of the mechanical blind hole, and a fourth conductive layer is deposited on the inner wall surface of the through hole, a second pulse electroplating process is used to deposit a fifth conductive layer on the inner wall surface of the mechanical blind hole, and before a sixth conductive layer is deposited on the inner wall surface of the through hole, the method further includes: The laser blind via is filled with a hole filling process to ensure the electroplating quality of the laser blind via; After the fifth conductive layer is deposited on the inner wall surface of the mechanical blind hole by using the second pulse electroplating process and the sixth conductive layer is deposited on the inner wall surface of the through hole by using the third pulse electroplating process and before the seventh conductive layer is deposited on the inner wall surface of the through hole by using the third pulse electroplating process, the method further includes: The mechanical blind holes are filled with a hole filling process to ensure the electroplating quality of the mechanical blind holes.

10. A circuit board, characterized in that: The circuit board is prepared by the electroplating method of any one of claims 1 to 9.