Hydrogenation catalyst as well as preparation method and application thereof
Through the catalyst of Cu nanoparticles and Zn(Al)O composite oxide support, the contradiction between conversion and selectivity of existing catalysts under low temperature and low pressure is solved, and the selection of hydrogenation of CO2 to methanol and butadiene is achieved. Efficient catalysis reduces costs and improves stability.
Patent Information
- Application Number
- CN202310557172.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-17
AI Technical Summary
In the process of selective hydrogenation of CO2 to methanol and butadiene, there is a contradiction between conversion and selectivity of existing catalysts, and the stability and cost of Pd-based catalysts are difficult to achieve efficient catalysis at low temperatures and low pressures.
The catalyst using Cu nanoparticles and Zn(Al)O composite oxide support is used. The surface of Cu nanoparticles has grain boundaries and ZnOx cladding. It is prepared by reducing the CuZnAl-LDHs precursor under a hydrogen atmosphere to achieve the low-temperature and low-pressure activity of the catalyst and Selective improvement.
While achieving CO2 conversion and methanol selectivity at low temperature and low pressure, the catalyst is cheap and stable in performance, and is suitable for selective hydrogenation of butadiene, achieving high conversion and high selectivity.
Smart Images

Figure CN118988327A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of hydrogenation catalysts, and specifically relates to a hydrogenation catalyst and a preparation method thereof, as well as application of the catalyst in CO2 hydrogenation to methanol and butadiene selective hydrogenation. Background Art
[0002] The CO2 hydrogenation to methanol reaction is one of the important ways to convert and utilize CO2. Methanol is a basic organic chemical raw material with a wide range of uses. It can be used in chemical products such as synthetic fibers, formaldehyde, plastics, medicines, pesticides, dyes, synthetic proteins, and can also be used as a liquid fuel for direct methanol fuel cells and improved diesel engines.
[0003] ZnO-Al2O3 oxide-supported Cu catalyst has good selectivity and stability and has been industrially applied in CO2 hydrogenation to methanol. However, while high conversion rates can be achieved under high temperature and high pressure conditions, there is competition for the production of CO by the reverse water gas shift reaction. For methanol synthesis, there is a "seesaw" effect between conversion rate and selectivity. The reaction temperature of the catalyst commonly used for CO2 hydrogenation to methanol is about 250-350℃, and the reaction pressure is about 6-8MPa. Under low temperature and low pressure conditions, the catalyst activity and selectivity will decrease significantly. Therefore, it is very necessary to prepare a catalyst that can simultaneously improve CO2 conversion rate and methanol selectivity at low temperature and low pressure.
[0004] The catalyst commonly used in industry for selective hydrogenation to remove a small amount of 1,3-butadiene in naphtha cracking products is a Pd-based catalyst. Since the generated butene will be further hydrogenated to form butane, it is difficult to maximize the utilization of raw materials. For example, patent document CN109092302B mentions that Pd nanoparticles are loaded on an alumina carrier, and the loading amount of Pd is 0.5wt%. When the conversion rate of 1,3-butadiene is close to 100%, the original 1-butene in the reaction gas is also slightly lost. The stability of Pd-based monometallic catalysts is relatively poor, and the formation of hydrocarbons and carbon deposits in the reaction can easily deactivate the catalyst. Therefore, a second metal is added to improve the butene selectivity of the supported Pd nanocatalyst. However, the reaction activity decreases after the addition of the second metal. For example, patent document CN109092302B mentions that PdLa (or PdCe, PdLaCe) nanoparticles are loaded on an alumina carrier. At 40°C, when 1,3-butadiene is nearly completely converted, the original 1-butene in the reaction gas also has a slight loss of about 3%, and the selectivity improvement is very limited. The 1-butene in the original reaction gas is also hydrogenated.
[0005] Pd-based catalysts have been widely used in the industrial C4 fraction selective hydrogenation process, but the scarcity of resources and high prices have become bottlenecks for the large-scale application of Pd-based catalysts. Therefore, the research team is also committed to developing non-precious metal-based catalysts to replace precious metal Pd-based catalysts. Summary of the invention
[0006] Based on the above situation, the purpose of the present invention is to provide a hydrogenation catalyst and its preparation method and application, the catalyst exhibits excellent CO2 conversion rate and methanol selectivity at low temperature and low pressure, and the CO2 conversion rate and methanol selectivity can be improved at the same time; the catalyst is used for selective hydrogenation of butadiene, the butadiene conversion rate and butene selectivity are high, and the performance is stable.
[0007] The first aspect of the present invention provides a hydrogenation catalyst, which contains Cu nanoparticles and a Zn(Al)O composite oxide carrier. The Cu nanoparticles have grain boundaries on their surfaces and a ZnOx coating layer, 0<x<1.
[0008] The second aspect of the present invention provides a method for preparing the above-mentioned hydrogenation catalyst, the preparation method comprising:
[0009] 1) Preparation of catalyst precursor CuZnAl-LDHs;
[0010] 2) reducing CuZnAl-LDHs in a hydrogen atmosphere to obtain a catalyst, wherein the reduction conditions include: heating to 400-460° C. at a rate of 1-5° C. / min, maintaining the temperature for 5-30 min, and then immediately cooling.
[0011] The third aspect of the present invention provides the use of the above catalyst in the production of methanol by hydrogenation of CO2.
[0012] The fourth aspect of the present invention provides the use of the above catalyst in the selective hydrogenation of butadiene.
[0013] Compared with the prior art, the advantages of the present invention are:
[0014] 1. The catalyst of the present invention is used for producing methanol by hydrogenation of CO2, has a higher conversion rate and selectivity at a lower pressure and temperature, and can simultaneously improve the conversion rate and selectivity, thereby achieving a high yield of methanol.
[0015] 2. The catalyst of the present invention is used for the selective hydrogenation of butadiene. The catalyst is low in price and has a relatively good conversion rate and selectivity and stable performance.
[0016] 3. The catalyst of the present invention can be obtained by direct reduction of a hydrotalcite precursor, and the preparation method is simple. The surface defects of the nanoparticles are induced by the different chemical microenvironments of the active metals in the hydrotalcite layer, and a supported catalyst with grain boundaries and a ZnOx coating layer on the surface of the Cu nanoparticles can be obtained.
[0017] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 : Butadiene conversion rate of each catalyst at different temperatures.
[0019] Figure 2 : Butadiene conversion rate of each catalyst and the corresponding butene selectivity. DETAILED DESCRIPTION
[0020] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0021] According to a first aspect of the present invention, the present invention provides a hydrogenation catalyst comprising Cu nanoparticles and a Zn(Al)O composite oxide carrier, wherein the Cu nanoparticles have grain boundaries on their surfaces and a ZnOx coating layer, 0<x<1.
[0022] In the present invention, based on the total weight of the catalyst, the loading amount of the Cu nanoparticles may be 8.0 to 30.0 wt%, preferably 10.0 to 25.0 wt%.
[0023] According to the present invention, the particle size of the Cu nanoparticles may be 2 to 8 nm, preferably 3 to 5 nm.
[0024] In the present invention, it is confirmed by XPS detection that ZnOx is a mixture, 0<x<1.
[0025] According to a second aspect of the present invention, the present invention provides a method for preparing the above-mentioned hydrogenation catalyst, the preparation method comprising:
[0026] 1) Preparation of catalyst precursor CuZnAl-LDHs;
[0027] 2) reducing CuZnAl-LDHs in a hydrogen atmosphere to obtain a catalyst, wherein the reduction conditions include: heating to 400-460° C. at a rate of 1-5° C. / min, maintaining the temperature for 5-30 min, and then immediately cooling.
[0028] In the present invention, the CuZnAl-LDHs can be prepared by conventional methods in the prior art, such as a constant pH method, which specifically includes the following steps:
[0029] (1) Cu 2+ 、Zn 2+ 、Al 3+ Prepare a salt solution, and prepare an alkaline solution by mixing Na2CO3 and NaOH; drip the salt solution and the alkaline solution into a stirred reaction vessel, and control the pH of the reaction solution to be 9.5±0.2. After the salt solution is dripped, the reaction solution is crystallized at a constant temperature of 60-80°C for 10-30h;
[0030] (2) The reaction product was filtered, washed with deionized water, and dried to obtain CuZnAl-LDHs.
[0031] Other specific parameters in the above steps can be selected with reference to the prior art. In order to obtain CuZnAl-LDHs with better crystal form, preferably, in the salt solution, (Cu 2+ +Zn 2+ )∶Al 3+ The molar ratio of Cu is 3:1. 2+ ∶Zn 2+ The molar ratio of Cu = 1:1-10, Cu 2+ 、Zn 2+ and Al 3+ The total molar concentration is 0.1-1 mol / L.
[0032] Preferably, in the alkaline solution, the molar concentration of Na2CO3 may be 0.05-0.5 mol / L, and the molar concentration of NaOH may be 0.1-0.8 mol / L.
[0033] According to the present invention, the stirring speed, drying temperature, etc. of the reaction container can be conventionally selected, such as the stirring speed can be 200-600 r / min, and the drying temperature can be 60-80°C.
[0034] According to the third aspect of the present invention, the present invention provides the use of the above catalyst in CO2 hydrogenation to produce methanol.
[0035] According to the present invention, the reaction conditions for preparing methanol by hydrogenation of CO2 include: a reaction temperature of 150-240°C; a reaction pressure of 1.5-2.5 MPa; a reaction feed composition of CO2:H2:Ar=15-20:65-75:4 in volume ratio; a volume space velocity of 3000-8000 h -1 , the catalyst dosage is 0.50-2.0g.
[0036] According to a fourth aspect of the present invention, the present invention provides use of the above catalyst in the selective hydrogenation of butadiene.
[0037] According to the present invention, the reaction conditions for the selective hydrogenation of butadiene include: a reaction temperature of 20 to 150° C.;
[0038] The reaction pressure is 0.1 MPa; the reaction feed composition is butadiene: hydrogen: argon = 1: 3-8: 40-50 in volume ratio; the volume space velocity is 3000-8000 h -1 , the catalyst dosage is 0.10-2.0g.
[0039] In the present invention, whether it is the CO2 hydrogenation to methanol reaction or the butadiene selective hydrogenation reaction, the catalyst is pre-reduced before use, and the pre-reduction conditions include: reduction at 250-350°C for 0.5-1h in a hydrogen atmosphere.
[0040] The substances and parameters not limited in the present invention can be selected according to the existing technology and belong to the conventional technical means in this field.
[0041] The present invention will be further described below with reference to the following examples, but is not limited to these examples.
[0042] Example 1
[0043] Step A: Accurately weigh 15mmol Cu(NO3)2·3H2O, 52.5mmol Zn(NO3)2·6H2O and 22.5mmol Al(NO3)3·9H2O, put them into a beaker filled with 200mL deionized water, stir until completely dissolved, and obtain a salt solution; weigh 45mmol Na2CO3 and 126mmol NaOH, put them into a beaker filled with 200mL deionized water, stir until completely dissolved, and obtain an alkaline solution. Place 200mL deionized water in a 1000mL four-necked flask. Stir at room temperature at 300r / min, and drop the salt solution and the alkaline solution into the four-necked flask drop by drop, and control the pH value to 9.5. After the salt solution is completely dripped, crystallize at a constant temperature of 65℃ in a water bath for 24h. After vacuum filtration, obtain a solid sample, wash with deionized water, and then dry in an oven at 70℃, grind to obtain Cu2Zn7Al3-LDHs powder, and dry and store.
[0044] Step B: The Cu2Zn7Al3-LDHs prepared above was reduced in a hydrogen atmosphere. The reduction procedure was as follows: heating from room temperature to 450°C at a heating rate of 2°C / min, keeping the temperature for 10 min, and then immediately cooling down to obtain a supported Cu nanoparticle catalyst 11.2ZnO x / Cu-Zn(Al)O.
[0045] ICP detection showed that the actual loading amount of Cu nanoparticles in the catalyst was 11.2wt%. Transmission electron microscopy showed that the surface of the Cu nanoparticles had two grain boundaries and a ZnOx coating layer, and the particle size of the Cu nanoparticles was 3.7nm.
[0046] Example 2
[0047] Step A: Accurately weigh 22.5mmol Cu(NO3)2·3H2O, 45.0mmol Zn(NO3)2·6H2O and 22.5mmol Al(NO3)3·9H2O, put them into a beaker filled with 200mL deionized water, stir until completely dissolved, and obtain a salt solution; weigh 45mmol Na2CO3 and 126mmol NaOH, put them into a beaker filled with 200mL deionized water, stir until completely dissolved, and obtain an alkaline solution. Place 200mL deionized water in a 1000mL four-necked flask. Stir at room temperature at 300r / min, and drop the salt solution and the alkaline solution into the four-necked flask drop by drop, and control the pH value to 9.5. After the salt solution is completely dripped, crystallize at a constant temperature of 65℃ in a water bath for 24h. After vacuum filtration, obtain a solid sample, wash with deionized water, and then dry in an oven at 70℃, grind to obtain Cu3Zn6Al3-LDHs powder, and dry and store.
[0048] Step B: The Cu3Zn6Al3-LDHs prepared above was reduced in a hydrogen atmosphere. The reduction procedure was as follows: heating from room temperature to 450°C at a heating rate of 2°C / min, keeping the temperature for 10 min, and then immediately cooling down to obtain a supported Cu nanoparticle catalyst 16.8ZnO x / Cu-Zn(Al)O.
[0049] ICP detection showed that the actual loading amount of Cu nanoparticles in the catalyst was 16.8wt%. Transmission electron microscopy showed that the surface of the Cu nanoparticles had three grain boundaries and a ZnOx coating layer, and the particle size of the Cu nanoparticles was 4.2nm.
[0050] Example 3
[0051] Step A: Accurately weigh 30.0mmol Cu(NO3)2·3H2O, 37.5mmol Zn(NO3)2·6H2O and 22.5mmol Al(NO3)3·9H2O, put them into a beaker filled with 200mL deionized water, stir until completely dissolved, and obtain a salt solution; weigh 45mmol Na2CO3 and 126mmol NaOH, put them into a beaker filled with 200mL deionized water, stir until completely dissolved, and obtain an alkaline solution. Place 200mL deionized water in a 1000mL four-necked flask. Stir at room temperature at 300r / min, and drop the salt solution and the alkaline solution into the four-necked flask drop by drop, and control the pH value to 9.5. After the salt solution is completely dripped, crystallize at a constant temperature of 65℃ in a water bath for 24h. After vacuum filtration, obtain a solid sample, wash with deionized water, and then dry in an oven at 70℃, grind to obtain Cu4Zn5Al3-LDHs powder, and dry and store.
[0052] Step B: The Cu4Zn5Al3-LDHs prepared above was reduced in a hydrogen atmosphere. The reduction procedure was as follows: heating from room temperature to 450°C at a heating rate of 2°C / min, keeping the temperature for 10 min, and then immediately cooling down to obtain Cu nanoparticle catalyst 25.0ZnO x / Cu-Zn(Al)O.
[0053] ICP detection showed that the actual loading amount of Cu nanoparticles in the catalyst was 25.0wt%. Transmission electron microscopy showed that the surface of the Cu nanoparticles had five grain boundaries and a ZnOx coating layer, and the particle size of the Cu nanoparticles was 4.5nm.
[0054] Comparative Example 1
[0055] Step A: Same as Example 1.
[0056] Step B: The prepared Cu2Zn7Al3-LDHs was reduced in a hydrogen atmosphere. The reduction procedure was as follows: heating from room temperature to 500°C at a heating rate of 2°C / min, keeping the temperature for 10 min and then immediately cooling down to obtain a supported Cu nanoparticle catalyst 11.2Cu-Zn(Al)O.
[0057] The actual loading amount of the Cu nanoparticles in the catalyst is 11.2wt%, the surface of the Cu nanoparticles has two grain boundaries but no ZnOx coating layer, and the particle size of the Cu nanoparticles is 3.8nm.
[0058] Comparative Example 2
[0059] Step A: Same as Example 2.
[0060] Step B: The prepared Cu3Zn6Al3-LDHs was reduced in a hydrogen atmosphere. The reduction procedure was as follows: heating from room temperature to 500°C at a heating rate of 2°C / min, keeping the temperature for 10 min and then immediately cooling down to obtain a supported Cu nanoparticle catalyst 16.8Cu-Zn(Al)O.
[0061] The actual loading amount of the Cu nanoparticles in the catalyst is 16.8wt%, the surface of the Cu nanoparticles has three grain boundaries but no ZnOx coating layer, and the particle size of the Cu nanoparticles is 4.2nm.
[0062] Comparative Example 3
[0063] Step A: Same as Example 3.
[0064] Step B: The prepared Cu4Zn5Al3-LDHs was reduced in a hydrogen atmosphere. The reduction procedure was as follows: heating from room temperature to 500°C at a heating rate of 2°C / min, keeping the temperature for 10 min, and immediately cooling down to obtain a supported Cu nanoparticle catalyst 25.0Cu-Zn(Al)O.
[0065] The actual loading amount of the Cu nanoparticles in the catalyst is 25.0wt%, the surface of the Cu nanoparticles has five grain boundaries but no ZnOx coating layer, and the particle size of the Cu nanoparticles is 4.6nm.
[0066] Comparative Example 4
[0067] Step A: Accurately weigh 67.5mmol Zn(NO3)2·6H2O and 22.5mmol Al(NO3)3·9H2O, put them into a beaker filled with 200mL deionized water, stir until completely dissolved, and obtain a salt solution; weigh 45mmol Na2CO3 and 126mmol NaOH, put them into a beaker filled with 200mL deionized water, stir until completely dissolved, and obtain an alkaline solution. Place 200mL deionized water in a 1000mL four-necked flask. Stir at room temperature at 300r / min, and drop the salt solution and the alkaline solution into the four-necked flask drop by drop, and control the pH value to 9.5. After the salt solution is completely dripped, crystallize at a constant temperature of 65℃ in a water bath for 24h. After vacuum filtration, obtain a solid sample, wash with deionized water, and then dry in an oven at 70℃, grind to obtain ZnAl-LDHs powder, and dry and store.
[0068] Step B: The round-bottom flask containing the ZnAl-LDHs prepared in step (A) was impregnated with an equal volume of Cu(NO3)3·3H2O aqueous solution (concentration of 24wt%), shaken evenly for 30min, and dried at 120°C for 2h to obtain Cu / ZnAl-LDHs.
[0069] Step C: The Cu / ZnAl-LDHs prepared above were reduced in a hydrogen atmosphere. The reduction procedure was: heating from room temperature to 450°C at a heating rate of 2°C / min, keeping the temperature for 10 min, and then immediately cooling to obtain a supported Cu nanoparticle catalyst 24.8Cu / Zn(Al)O.
[0070] The actual loading amount of the Cu nanoparticles in the catalyst is 24.8wt%, there is no grain boundary and no ZnOx coating layer on the surface of the Cu nanoparticles, and the particle size of the Cu nanoparticles is 4.7nm.
[0071] The catalysts prepared in the embodiments and comparative examples were pressed into 20-40 mesh granular catalysts, which were loaded into a fixed bed reactor and pretreated by introducing H2 at a flow rate of 30 mL / min / g at 300°C for 0.5 h. After cooling to 200°C, reaction feed was introduced for catalytic reaction at a reaction pressure of 2.0 MPa. In terms of volume ratio, the reaction feed composition was CO2:H2:Ar=24:72:4. The flow rate was 100 mL / min, and the volume space velocity (GHSV) was 6000 h -1 The amount of catalyst used was 1.0 g. The reaction tail gas was connected to a gas chromatograph for quantitative analysis, and the conversion rate of CO2 and the selectivity of CH3OH were calculated. The specific reaction catalytic performance is shown in Table 1.
[0072] Table 1
[0073]
[0074] It can be seen from Table 1 that the use of the catalyst of the present application has a higher conversion rate and selectivity for producing methanol by hydrogenation of CO2 at low temperature and low pressure, and can achieve simultaneous improvement in conversion rate and selectivity.
[0075] The catalysts prepared in the examples and comparative examples were pressed into 20-40 mesh granular catalysts, which were loaded into a fixed bed reactor, and H2 was introduced for pretreatment at a flow rate of 30 mL / min / g at 300°C for 0.5 h. After cooling to room temperature of 20°C, reaction feed was introduced for catalytic reaction at a pressure of 0.1 MPa under normal pressure, and the composition of the reaction feed was 1,3-butadiene: H2: Ar = 2: 10: 88; the flow rate was 50 mL / min, and the GHSV was 6000 h -1 The catalyst dosage was 0.25 g, and the conversion rate of butadiene and the selectivity of butene were measured at different reaction temperatures. The reaction tail gas was connected to a gas chromatograph for quantitative analysis. The conversion rate of butadiene and the selectivity of butene, and the catalytic performance of the 1,3-butadiene hydrogenation reaction were as follows: Figure 1 , Figure 2 shown.
[0076] Depend on Figure 1 , Figure 2 It can be seen that the catalyst of the present application is used for the selective hydrogenation of butadiene, and the conversion rate can reach 100% at 0.1 MPa and a relatively low reaction temperature, and the butene selectivity and stability are also relatively high.
[0077] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A hydrogenation catalyst, characterized in that The catalyst contains Cu nanoparticles and a Zn(Al)O composite oxide carrier. The surface of the Cu nanoparticles has a grain boundary and a ZnOx coating layer, and 0<x<1.
2. The hydrogenation catalyst according to claim 1, wherein Based on the total weight of the catalyst, the loading amount of the Cu nanoparticles is 8.0 to 30.0 wt%, preferably 10.0 to 25.0 wt%.
3. The hydrogenation catalyst according to claim 1, wherein The particle size of the Cu nanoparticles is 2 to 8 nm, preferably 3 to 5 nm.
4. The method for preparing the hydrogenation catalyst according to any one of claims 1 to 3, characterized in that: The preparation method comprises: 1) Preparation of catalyst precursor CuZnAl-LDHs; 2) reducing CuZnAl-LDHs in a hydrogen atmosphere to obtain a catalyst, wherein the reduction conditions include: heating to 400-460° C. at a rate of 1-5° C. / min, maintaining the temperature for 5-30 min, and then immediately cooling.
5. The method for preparing a hydrogenation catalyst according to claim 4, wherein: The CuZnAl-LDHs are prepared by a constant pH method, comprising the following steps: (1) Cu 2+ 、Zn 2+ 、Al 3+ Prepare a salt solution, and prepare an alkaline solution by mixing Na2CO3 and NaOH; drip the salt solution and the alkaline solution into a stirred reaction vessel, and control the pH of the reaction solution to be 9.5±0.
2. After the salt solution is dripped, the reaction solution is crystallized at a constant temperature of 60-80°C for 10-30h; (2) filtering the reaction product, washing with deionized water, and drying to obtain CuZnAl-LDHs; Preferably, in the salt solution, (Cu 2+ +Zn 2+ )∶Al 3+ The molar ratio of Cu is 3:
1. 2+ ∶Zn 2+ The molar ratio of Cu = 1:1-10, Cu 2+ 、Zn 2+ and Al 3+ The total molar concentration is 0.1-1 mol / L; Preferably, in the alkaline solution, the molar concentration of Na2CO3 is 0.05-0.5 mol / L, and the molar concentration of NaOH is 0.1-0.8 mol / L.
6. Use of the catalyst according to any one of claims 1 to 3 in the production of methanol by hydrogenation of CO2.
7. The use according to claim 6, wherein: The reaction conditions for CO2 hydrogenation to methanol include: reaction temperature of 150-240°C; reaction pressure of 1.5-2.5 MPa; reaction feed composition of CO2:H2:Ar=15-20:65-75:4 in volume ratio; volume space velocity of 3000-8000 h -1 , the catalyst dosage is 0.50-2.0g.
8. Use of the catalyst according to any one of claims 1 to 3 in the selective hydrogenation of butadiene.
9. The use according to claim 8, wherein: The reaction conditions for the selective hydrogenation of butadiene include: a reaction temperature of 20 to 150°C; a reaction pressure of 0.1 MPa; a reaction feed composition of butadiene: hydrogen: argon = 1:3 to 8:40 to 50 in volume ratio; a volume space velocity of 3000 to 8000 h -1 , the catalyst dosage is 0.10-2.0g.
10. The use according to claim 6 or 8, wherein: The catalyst is pre-reduced before use, and the pre-reduction conditions include: reduction at 250-350° C. for 0.5-1 h in a hydrogen atmosphere.
Citation Information
Patent Citations
Highly dispersed CuZnTi catalyst for hydrogenation of catalytic maleic anhydride to gamma-butyrolactone and preparation method thereof
CN101940927A
Processing method of catalytic hydrogenation of olefin-containing exhaust gas
CN105037064A
Catalyst for preparing methyl alcohol by adding hydrogen to CO2 and preparation method and application of catalyst
CN106563454A
Methanol / ethanol cross C-C bond coupling catalyst and preparation method thereof
CN110227471A
Preparation method of copper-based catalyst with copper-coated zinc oxide interface and application of copper-based catalyst in low-temperature catalysis of water gas shift reaction
CN114824320A