Method for directionally separating and recycling lithium and sodium in lithium hydroxide evaporation mother liquor
Through phosphate precipitation method and resin adsorption technology, efficient directional separation and recovery of lithium sodium resources is achieved in the evaporated mother liquor of lithium hydroxide, solving the problems of unrecovered sodium resources and waste in the existing technology, and improving product quality and economic benefits.
Patent Information
- Application Number
- CN202411115064.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The prior art fails to effectively recover sodium resources in the treatment of lithium hydroxide evaporation mother liquor, resulting in waste of resources and high cost. The consumption of carbon dioxide under high alkalinity is too large, affecting the preparation efficiency of lithium carbonate.
The lithium sodium resource is recovered by phosphate precipitation method. After heating and stirring, phosphate is added, followed by solid-liquid separation, dephosphorization and evaporation and crystallization treatment, combined with resin adsorption and calcium removal, and finally obtain high-purity lithium phosphate, sodium hydroxide and phosphoric acid. Calcium products realize directional separation and recovery of lithium sodium.
It improves lithium recycling rate and product quality, reduces water resource consumption and outsourcing costs, significantly improves economic benefits, and reduces the outsourcing costs of dephosphorizer and water through recycling and utilization.
Smart Images

Figure CN118993002A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium extraction from salt lakes, and in particular to a method for directional separation and recovery of lithium and sodium in lithium hydroxide evaporation mother liquor. Background Art
[0002] LiOH·H2O is one of the key raw materials for the production of lithium batteries and has a huge market. At present, the preparation of LiOH generally involves first preparing a pure lithium-containing solution through pretreatment, then causticizing or electrolyzing to produce a pure LiOH solution, and finally evaporating, crystallizing, washing, and drying to produce the LiOH·H2O product. The evaporation and crystallization process is accompanied by the production of a by-product, the evaporation mother liquor. The evaporation mother liquor has the characteristics of rich lithium and sodium resources, a high sodium-lithium ratio, and high alkalinity. The lithium and sodium contents are 12-20g / L and 150-300g / L, respectively, and it has huge economic value and recovery potential. At present, there are few reports on the treatment methods for lithium hydroxide evaporation mother liquor, and the mainstream treatment process mainly focuses on Li + The recycling of the wastewater is carried out without recycling the sodium resources.
[0003] CN115571901A discloses a method for preparing lithium carbonate by using the mother liquor evaporated from a salt lake to extract lithium. The method first dilutes the mother liquor with pure water to meet the feed requirements of the back-end membrane treatment, and then removes suspended matter, colloidal macromolecules, and divalent ions such as calcium and magnesium through ultrafiltration and nanofiltration in sequence. The battery-grade lithium carbonate product is then produced after two-stage carbonization-pyrolysis, solid-liquid separation, washing, drying, and demagnetization. In this method, due to the high alkalinity of the evaporated mother liquor, the two-stage carbonization to prepare the lithium bicarbonate solution results in excessive carbon dioxide consumption. If the mother liquor is directly carbonized to produce the lithium carbonate solution, the consumption of a large amount of carbon dioxide can be reduced, saving costs. In the subsequent process, due to the Na in the pyrolysis solution, the production of lithium carbonate solution is very expensive. + The content is high and it is difficult to meet battery-grade requirements after simple washing. In addition, the sodium resources are not recycled, resulting in a large amount of resources being wasted. Summary of the invention
[0004] In view of the deficiencies of the prior art, the present invention aims to provide a method for directional separation and recovery of lithium and sodium in lithium hydroxide evaporation mother liquor.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A method for directional separation and recovery of lithium and sodium in lithium hydroxide evaporation mother liquor comprises the following steps:
[0007] S1, heating the lithium hydroxide evaporation mother liquor and maintaining a constant temperature and stirring, then adding phosphate and continuing to stir the reaction; after the reaction is completed, solid-liquid separation is performed to obtain a crude lithium phosphate solid and a lithium precipitated liquid, and the crude lithium phosphate is washed with pure water, filtered and dried to obtain a lithium phosphate product;
[0008] S2, adding calcium-containing materials to the lithium precipitation liquid obtained in step S1, filtering to obtain a crude calcium phosphate solid and a dephosphorized liquid, and washing the crude calcium phosphate solid with pure water, filtering and drying to obtain a calcium phosphate product;
[0009] S3, the dephosphorized liquid obtained in step S2 is decalcified by resin adsorption to remove the residual Ca + , obtaining a decalcified liquid; desorbing the adsorbed resin to obtain a calcium-containing desorption liquid;
[0010] S4, evaporating and crystallizing the decalcified liquid obtained in step S3, returning the evaporated fresh water to wash the crude lithium phosphate and crude calcium phosphate, filtering the remaining slurry to obtain crude sodium hydroxide solid and mixed alkali, and washing, filtering and drying the crude sodium hydroxide to obtain a solid sodium hydroxide product.
[0011] Further, in step S1, the phosphate includes one or more of sodium phosphate, disodium hydrogen phosphate, and sodium dihydrogen phosphate, and the amount of phosphate added is the amount of all Li + 1-1.5 times the theoretical mass of phosphate required.
[0012] Furthermore, in step S1, the lithium hydroxide evaporation mother liquor is heated to 70-90° C. and then kept at a constant temperature and stirred, and then phosphate is added and the stirring reaction is continued for 1-3 hours.
[0013] Furthermore, the lithium phosphate product obtained in step S1 meets the Li2PO4-3 grade standard in the "YS / T 637-2022" standard, and is used to prepare high-purity lithium phosphate, battery-grade lithium carbonate and / or as a raw material product for battery-grade lithium hydroxide monohydrate.
[0014] Furthermore, in step S2, the amount of calcium-containing material added is calculated based on the calcium contained therein, and the amount of calcium added is 1-1.2 times the theoretical mass of calcium required to remove all phosphorus in the solution after lithium precipitation.
[0015] Furthermore, the calcium phosphate product obtained in step S2 has a purity of ≥98%, and can be used as a fertilizer or as a raw material product of food-grade calcium phosphate.
[0016] Furthermore, in step S3, the resin adsorption decalcification is performed using one or a combination of a fixed bed system and a continuous ion exchange system.
[0017] Furthermore, in step S4, the evaporation weight loss rate of evaporation crystallization is 40%-80%.
[0018] Furthermore, the solid sodium hydroxide product obtained in step S4 meets the IS-IT-Ⅰ type Ⅰ grade qualified product index in "GB 209-2006 Sodium Hydroxide for Industrial Use".
[0019] Furthermore, the calcium-containing material includes one or more of the calcium-containing desorption liquid produced in step S2, calcium chloride hexahydrate solid produced in the brine salt drying stage in the lithium extraction process of a salt lake enterprise that produces lithium carbonate and lithium hydroxide monohydrate, and dialysis nanofiltration calcium-containing concentrated water produced in the nanofiltration membrane calcium and magnesium removal stage.
[0020] The beneficial effects of the present invention are as follows: the present invention firstly adopts a phosphate precipitation method to recover Li in the evaporated mother liquor. + , and then the post-lithium precipitation liquid is dephosphorized and evaporated and crystallized to produce high-quality lithium phosphate, solid sodium hydroxide and calcium phosphate products. The process has a high lithium recovery rate and is simple and efficient. Compared with the traditional secondary lithium-containing solution treatment method, the present invention realizes the efficient directional separation and recovery of lithium and sodium resources in the evaporated mother liquor, rather than just recovering lithium resources. At the same time, the crude lithium phosphate and crude calcium phosphate washing adopts the subsequent evaporation and crystallization stage to produce fresh water. Therefore, the method of the present invention can significantly improve the economic benefits of the enterprise, and at the same time can greatly reduce the cost of purchasing caustic soda flakes and save water resources, and has high economic efficiency. In addition, the dephosphorization agent can come from the calcium-containing desorption liquid produced in the decalcification stage, and can also be used, such as the hexahydrate calcium chloride solid produced in the lake brine salt drying stage in the main lithium extraction process of the salt lake enterprise producing lithium carbonate and monohydrate lithium hydroxide, and the dialysis nanofiltration calcium-containing concentrated water produced in the nanofiltration membrane calcium and magnesium removal section. The main system outputs calcium-containing materials, thereby reducing the cost of purchasing the dephosphorization agent, and also improving the adaptability of the method of the present invention to the main production system. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a process flow chart of Examples 1-3 of the present invention. DETAILED DESCRIPTION
[0022] The present invention will be further described below in conjunction with the accompanying drawings. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to this embodiment.
[0023] Example 1
[0024] The raw material is lithium hydroxide evaporation mother liquor produced by a salt lake enterprise. Its main chemical components are: Li 14.9g / L, Na 173.0g / L, K 16.3g / L, OH - 13.4mol / L, this embodiment performs lithium and sodium directional separation and recovery on the evaporated mother liquor, such as Figure 1 As shown, the following steps are included:
[0025] (1) firstly heating the mother liquor of lithium hydroxide evaporation to 70° C., then maintaining the constant temperature and stirring, then adding 1.5 times the theoretical amount of sodium phosphate to the mother liquor of lithium hydroxide evaporation to precipitate lithium, and continuing to maintain the constant temperature and stirring for 1 hour after the addition, and performing solid-liquid separation after the stirring to obtain crude lithium phosphate and a solution after lithium precipitation, the lithium recovery rate of the process is 93.8%, and the crude lithium phosphate is washed, filtered, and dried to obtain a lithium phosphate product;
[0026] (2) Adding a calcium-containing material to the lithium precipitation liquid obtained in step (1) for dephosphorization, wherein the calcium-containing material is the calcium-containing desorption liquid produced in step (3), and the amount of calcium added is 1.2 times the theoretical amount. After filtering, crude calcium phosphate and dephosphorized liquid are obtained, and the phosphorus precipitation rate is 99.4%. The crude calcium phosphate is washed with pure water, filtered, and dried to obtain a calcium phosphate product with a purity of 98.16%;
[0027] (3) The dephosphorized liquid produced in step (2) is fed to a resin for decalcification to obtain a decalcified liquid and a calcium-containing desorption liquid. The decalcified liquid Ca + Mg + When the concentration is less than 0.05 mg / L, the calcium-containing desorption solution is returned to step (2) for dephosphorization;
[0028] (4) The decalcified liquid produced in step (3) is evaporated and crystallized, and the evaporation weight loss rate is 79.1%. The fresh water produced by evaporation is returned for washing crude lithium phosphate and crude calcium phosphate. The slurry is filtered to obtain crude sodium hydroxide solid and mixed alkali. The crude sodium hydroxide is washed, filtered, and dried to obtain a solid sodium hydroxide product.
[0029] Example 2
[0030] The raw material is lithium hydroxide evaporation mother liquor produced by a salt lake enterprise. Its main chemical components are: Li 14.9g / L, Na 173.0g / L, K 16.3g / L, OH - 13.4mol / L. In this embodiment, lithium and sodium are directional separated and recovered from the evaporated mother liquor. Figure 1 As shown, the following steps are included:
[0031] (1) firstly heating the mother liquor of lithium hydroxide evaporation to 90° C., then maintaining the constant temperature and stirring, then adding 1 times the theoretical amount of disodium hydrogen phosphate to the mother liquor of lithium hydroxide evaporation to precipitate lithium, and continuing to maintain the constant temperature and stirring for 3 hours after the addition is completed, and performing solid-liquid separation after the stirring is completed to obtain crude lithium phosphate and a solution after lithium precipitation, the lithium recovery rate of the process is 95.4%, and the crude lithium phosphate is washed, filtered, and dried to obtain a lithium phosphate product;
[0032] (2) adding a calcium-containing material to the lithium precipitation liquid obtained in step (1) for dephosphorization, wherein the calcium-containing material includes the calcium-containing desorption liquid produced in step (3) and the dialysis nanofiltration calcium-containing concentrated water produced by the lithium-containing brine nanofiltration membrane calcium and magnesium removal process, the amount of calcium added is 1 times the theoretical amount, and after filtering, crude calcium phosphate and dephosphorized liquid are obtained, and the phosphorus precipitation rate is 99.0%. The crude calcium phosphate is washed with pure water, filtered, and dried to obtain a calcium phosphate product with a purity of 98.1%;
[0033] (3) The dephosphorized liquid produced in step (2) is sent to a resin for adsorption and decalcification to obtain a decalcified liquid and a calcium-containing desorption liquid. The decalcified liquid Ca + Mg + When the concentration is less than 0.05 mg / L, the calcium-containing desorption solution is returned to step (2) for dephosphorization;
[0034] (4) The decalcified liquid produced in step (3) is evaporated and crystallized, and the evaporation weight loss rate is 41.6%. The fresh water produced by evaporation is returned for washing crude lithium phosphate and crude calcium phosphate. The slurry is filtered to obtain crude sodium hydroxide solid and mixed alkali. The crude sodium hydroxide is washed, filtered, and dried to obtain a solid sodium hydroxide product.
[0035] Example 3
[0036] The raw material is lithium hydroxide evaporation mother liquor produced by a salt lake enterprise. Its main chemical components are: Li 17.1g / L, Na 148.0g / L, K 13.6g / L, OH - 11.7mol / L. In this embodiment, lithium hydroxide evaporation mother liquor is subjected to lithium and sodium directional separation and recovery, such as Figure 1 As shown, the following steps are included:
[0037] (1) firstly heating the mother liquor of lithium hydroxide evaporation to 85° C., then maintaining the constant temperature and stirring, then adding 1.3 times the theoretical amount of sodium dihydrogen phosphate to the mother liquor of lithium hydroxide evaporation to precipitate lithium, and continuing to maintain the constant temperature and stirring for 2 hours after the addition is completed, and performing solid-liquid separation after the stirring is completed to obtain crude lithium phosphate and a solution after lithium precipitation, and the lithium recovery rate of the process is 94.2%, and the crude lithium phosphate is washed and dried to obtain lithium phosphate;
[0038] (2) adding a calcium-containing material to the lithium precipitation liquid obtained in step (1) for dephosphorization, wherein the calcium-containing material includes the calcium-containing desorption liquid produced in step (3) and the calcium chloride hexahydrate solid produced in the brine salt drying stage, and the amount of calcium added is 1.15 times the theoretical amount, and filtering to obtain crude calcium phosphate and dephosphorized liquid, wherein the phosphorus precipitation rate is 99.3%, and the crude calcium phosphate is washed with pure water, filtered, and dried to obtain a calcium phosphate product with a purity of 98.7%;
[0039] (3) The dephosphorized liquid produced in step (2) is fed to a resin for decalcification to obtain a decalcified liquid and a calcium-containing desorption liquid. The decalcified liquid Ca + Mg + When the concentration is less than 0.05 mg / L, the calcium-containing desorption solution is returned to step (2) for dephosphorization;
[0040] (4) evaporating and crystallizing the decalcified liquid produced in step (3), wherein the weight loss rate of evaporation is 65.7%, and the fresh water produced by evaporation is returned to be used for washing crude lithium phosphate and crude calcium phosphate. After filtering the slurry, crude sodium hydroxide solid and mixed alkali are obtained, and the crude sodium hydroxide is washed, filtered, and dried to obtain a solid sodium hydroxide product;
[0041] The chemical compositions of the lithium phosphate product and the sodium hydroxide solid product produced in Examples 1-3 are shown in Table 1 and Table 2, respectively.
[0042] Table 1 Chemical composition of lithium phosphate products produced in Examples 1-3 / (%)
[0043]
[0044]
[0045] Table 2 Chemical composition of sodium hydroxide solid product produced by Example 1-3
[0046] Example 1 2 3 NaOH mass fraction / % 98.39 98.51 98.60 <![CDATA[Mass fraction of Na2CO3 / %]]> 0.33 0.42 0.15 NaCl mass fraction / % 0.02 0.02 0.04 <![CDATA[Mass fraction of Fe2O3 / %]]> 0.003 0.002 <0.001
[0047] For those skilled in the art, various corresponding changes and modifications can be made according to the above technical solutions and concepts, and all of these changes and modifications should be included in the protection scope of the claims of the present invention.
Claims
1. A method for directional separation and recovery of lithium and sodium from lithium hydroxide evaporation mother liquor, characterized in that: The steps include: S1, heating the lithium hydroxide evaporation mother liquor and maintaining a constant temperature and stirring, then adding phosphate and continuing to stir the reaction; after the reaction is completed, solid-liquid separation is performed to obtain a crude lithium phosphate solid and a lithium precipitated liquid, and the crude lithium phosphate is washed with pure water, filtered and dried to obtain a lithium phosphate product; S2, adding calcium-containing materials to the lithium precipitation liquid obtained in step S1, filtering to obtain a crude calcium phosphate solid and a dephosphorized liquid, and washing the crude calcium phosphate solid with pure water, filtering and drying to obtain a calcium phosphate product; S3, the dephosphorized liquid obtained in step S2 is decalcified by resin adsorption to remove the residual Ca + , obtaining a decalcified liquid; desorbing the adsorbed resin to obtain a calcium-containing desorption liquid; S4, evaporating and crystallizing the decalcified liquid obtained in step S3, returning the evaporated fresh water to wash the crude lithium phosphate and crude calcium phosphate, filtering the remaining slurry to obtain crude sodium hydroxide solid and mixed alkali, and washing, filtering and drying the crude sodium hydroxide to obtain a solid sodium hydroxide product.
2. The method according to claim 1, characterized in that In step S1, the phosphate includes one or more of sodium phosphate, disodium hydrogen phosphate, and sodium dihydrogen phosphate, and the amount of phosphate added is the amount of all Li + 1-1.5 times the theoretical mass of phosphate required.
3. The method according to claim 1, characterized in that In step S1, the mother liquor of lithium hydroxide evaporation is heated to 70-90°C and then kept at a constant temperature and stirred, and then phosphate is added and stirred to react for 1-3 hours.
4. The method according to claim 1, characterized in that: The lithium phosphate product obtained in step S1 meets the Li2PO4-3 grade standard in the "YS / T 637-2022" standard and is used to prepare high-purity lithium phosphate, battery-grade lithium carbonate and / or as a raw material product for battery-grade lithium hydroxide monohydrate.
5. The method according to claim 1, characterized in that In step S2, the amount of calcium-containing material added is calculated based on the calcium contained therein, and the amount of calcium added is 1-1.2 times the theoretical mass of calcium required to remove all phosphorus in the solution after lithium precipitation.
6. The method according to claim 1, characterized in that The calcium phosphate product obtained in step S2 has a purity of ≥98% and can be used as a fertilizer or as a raw material product of food-grade calcium phosphate.
7. The method according to claim 1, characterized in that In step S3, the resin adsorption decalcification is performed using one or a combination of a fixed bed system and a continuous ion exchange system.
8. The method according to claim 1, characterized in that In step S4, the evaporation weight loss rate of evaporation crystallization is 40%-80%.
9. The method according to claim 1, characterized in that: The solid sodium hydroxide product obtained in step S4 meets the IS-IT-Ⅰ type Ⅰ grade qualified product index in "GB 209-2006 Industrial Sodium Hydroxide".
10. The method according to claim 1, characterized in that In step S3, the calcium-containing material includes one or more of the calcium-containing desorption liquid produced in step S2, calcium chloride hexahydrate solid produced in the brine salt drying stage in the lithium extraction process of a salt lake enterprise that produces lithium carbonate and lithium hydroxide monohydrate, and dialysis nanofiltration calcium-containing concentrated water produced in the nanofiltration membrane calcium and magnesium removal stage.
Citation Information
Patent Citations
Method and system for preparing battery grade and high purity grade lithium hydroxide and lithium carbonate from high-impurity lithium sources
CA3077834A1
New technology for preparing lithium products from lepidolite leaching solution
CN109970085A
Method for efficiently utilizing high-purity lithium carbonate mother liquor
CN116281906A
Method for comprehensively utilizing phosphorus, aluminum and lithium elements in phosphorus-aluminum-lithium ore
CN116986615A
Method for preparing battery-grade lithium carbonate through reinforced carbonization short distance
CN117142499A