Carbon nanotube grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material and preparation method thereof
By introducing silicon carbon-nitrogen shell layer on the surface of the carbon fiber and growing radial carbon nanotubes, the problem of uneven distribution of carbon nanotubes in carbon fiber/phenolic resin composites is solved, the strength of the material and electromagnetic shielding performance are improved, and the efficiency of the Electromagnetic shielding effect.
Patent Information
- Application Number
- CN202411257914.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-09
AI Technical Summary
The electromagnetic shielding performance of existing carbon fiber/phenolic resin composites in the field of electromagnetic shielding is limited, and the growth quality of carbon nanotubes in catalytic chemical deposition is poor, making it difficult to be distributed at high density and uniformly, resulting in a decrease in material strength and electromagnetic shielding performance.
The silicon carbon-nitrogen shell layer is introduced on the surface of the carbon fiber, and radial carbon nanotubes are grown through catalytic chemical deposition to form a carbon nanotube grafted silicon carbon-nitrogen-carbon fiber/phenolic resin composite material, and high density is achieved through specific process steps design And evenly distributed carbon nanotubes.
The strength and electromagnetic shielding performance of carbon fiber/phenolic resin composite materials are improved, the uniform distribution of high-density carbon nanotubes is achieved, and the mechanical properties and electromagnetic shielding performance of the material are enhanced. The electromagnetic shielding performance reaches 40.73dB, and the tensile strength is significantly improved.
Smart Images

Figure CN118994842A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a silicon carbon nitrogen-carbon fiber composite material and a preparation method thereof, and in particular to a carbon nanotube grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material and a preparation method thereof. Background Art
[0002] Carbon fiber / phenolic resin composites are widely used in the field of electromagnetic shielding due to their light weight, high strength, corrosion resistance, easy processing and many other characteristics. However, due to the low electrical conductivity of phenolic resin, the electromagnetic shielding effectiveness of carbon fiber / phenolic resin composites is greatly limited. In addition, due to the chemical inertness and smoothness of the carbon fiber surface, the combination of carbon fiber and phenolic resin is prone to debonding. During the use of the composite material, stress concentration occurs due to the action of external forces, resulting in matrix fragmentation and composite material damage. If the electromagnetic shielding material breaks, wears, and ages during use, its electromagnetic interference shielding performance will be greatly reduced. Therefore, it is worth studying how to simultaneously improve the mechanical properties and electromagnetic shielding effectiveness of carbon fiber / phenolic resin composites.
[0003] Generally, the interfacial strength of electromagnetic shielding materials can be improved by introducing nanofillers. Carbon nanotubes are often introduced into electromagnetic shielding materials as conductive fillers due to their advantages such as light weight, high strength, high aspect ratio, and high thermal conductivity. However, the process of introducing carbon nanotubes into carbon fiber / phenolic resin composites by catalytic chemical deposition often has the following problems: metal catalysts are prone to react with carbon at high temperatures and diffuse to lose catalytic activity, and the ability of carbonaceous surfaces to capture and fix metal catalysts is weak, and the loaded metal particles are prone to move and agglomerate. Therefore, the growth quality of carbon nanotubes obtained on the surface of carbon fiber by catalytic chemical deposition is poor, mainly manifested in nanotube curling, disordered orientation and low density. Agglomeration will lead to poor polarization loss and poor impedance matching, resulting in poor absorption capacity. Therefore, how to introduce high-density and uniformly distributed carbon nanotubes into carbon fiber / phenolic resin composites deserves further study.
[0004] Literature 1 "Hui Qian, Alexander Bismarck, Emile S. Greenhalgh, Gerhard Kalinka, Milo SP Shaffer. Hierarchical composites reinforced with carbon nanotube grafted fibers: the potential assessed at the single fiber level. Chemistry of Materials, 2008, 20(5): 1862-1869." reported that curved carbon nanotubes were grown on the surface of carbon fibers, and the tensile strength of the composite material was increased by about 26%.
[0005] Reference 2 "Chao Chang, Xiu Yue, Bin Hao, Dan Xing, Peng-Cheng Ma. Improvement of the electromagnetic shielding properties of C / SiC composites by electrophoretic deposition of carbon nanotube on carbon fibers. Carbon, 2016, 109: 149-153." reported the introduction of carbon nanotubes into carbon fiber reinforced silicon carbide composites by electrophoretic deposition. The carbon nanotubes present a network structure, and the electromagnetic shielding effectiveness reaches 38.2 dB when the sample thickness is 3 mm.
[0006] Document 3 "Qiang Song, Kezhi Li, Hailiang Li, Hejun Li, Chang Ren. Grafting straight carbon nanotubes radially onto carbon fibers and their effect on the mechanical properties of carbon / carbon composites. Carbon, 2012, 50(10): 3949-3952." reported the preparation of upright oriented carbon nanotubes on the surface of carbon fibers. The carbon fibers were treated with strong acid immersion for 24 hours, and the carbon fibers were severely damaged and the density of carbon nanotubes was low.
[0007] However, the carbon nanotubes reported in the above literature are difficult to be distributed evenly and at high density on carbon fibers, and the strong acid treatment process will seriously damage the surface structure of the carbon fibers, resulting in a significant reduction in fiber strength. Therefore, it is difficult to introduce high-density and evenly distributed carbon nanotubes into composite materials without damaging the carbon fibers. Summary of the invention
[0008] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a carbon nanotube grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material and a preparation method thereof, which can make the carbon nanotubes on the carbon fiber high-density and uniformly distributed, and the material has high strength.
[0009] To achieve the above-mentioned purpose, the present invention discloses a method for preparing a carbon nanotube grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material, comprising the following steps: introducing a silicon carbon nitrogen shell layer on the surface of the carbon fiber, and then using a catalytic chemical deposition method to grow radial carbon nanotubes to obtain a carbon nanotube grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material.
[0010] Further, the method specifically includes the following steps:
[0011] 1) placing the carbon fiber cloth in a chemical vapor deposition furnace, heating it, and then using natural gas as a carbon source gas and argon as a protective gas for heat preservation to obtain sample A;
[0012] 2) uniformly mixing polysilazane and acetone to obtain solution B;
[0013] 3) Immerse sample A in solution B and place it at room temperature to obtain sample C;
[0014] 4) placing sample C in a tubular heat treatment furnace, heating it up and then keeping it warm, and taking out the sample after the temperature in the tubular heat treatment furnace cools down to room temperature to obtain sample D;
[0015] 5) Evenly mix ferrocene, anhydrous ethanol and ferrocene to obtain solution E;
[0016] 6) placing sample D in a tubular chemical vapor deposition furnace and heating it, injecting solution E into the tubular chemical vapor deposition furnace, and taking out the sample after the temperature in the tubular chemical vapor deposition furnace is cooled to room temperature, thereby obtaining sample F;
[0017] 7) uniformly mixing phenolic resin powder and anhydrous ethanol to obtain solution G;
[0018] 8) Soaking sample F in solution G, taking it out and drying it, and then leaving it at room temperature to obtain sample H;
[0019] 9) The sample H is subjected to hot pressing and curing to obtain a carbon nanotube grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material.
[0020] Further, the process of step 1) is:
[0021] The carbon fiber cloth was placed in a chemical vapor deposition furnace, the temperature was raised to 1000°C to 1100°C, natural gas was used as the carbon source gas with a flow rate of 0.8L / min to 1L / min, argon was used as the protective gas with a flow rate of 2.0L / min to 2.4L / min, and the temperature was kept for 2 to 4 hours to obtain sample A.
[0022] Further, in step 2), the mass ratio of polysilazane to acetone is 1:4 to 1:6;
[0023] In step 7), the mass ratio of phenolic resin powder to anhydrous ethanol is 1:3 to 1:2.
[0024] Furthermore, in step 5), the mass ratio of ferrocene to anhydrous ethanol is 1:80 to 1:100, and the mass ratio of ferrocene to ethylenediamine is 1:15 to 1:18.
[0025] Furthermore, the process of step 4) is: placing sample C in a tubular heat treatment furnace, heating it to 150°C~300°C and keeping it warm for 2~3 hours, then heating it to 800°C~950°C and keeping it warm for 2~3 hours, wherein the heating rate is 2.5°C / min~5°C / min, and taking out the sample after the temperature in the tubular heat treatment furnace cools to room temperature to obtain sample D.
[0026] Furthermore, the process of step 6) is: place sample D in a tubular chemical vapor deposition furnace, heat it to 800°C to 900°C, inject solution E into the tubular chemical vapor deposition furnace at a rate of 5ml / h to 15ml / h, and the injection time is 10 to 30 minutes. After the temperature in the tubular chemical vapor deposition furnace cools to room temperature, take out the sample to obtain sample F.
[0027] Furthermore, the process of step 8) is: soak sample F in solution G for 1 to 3 days, take it out and place it in an oven, heat it up and then keep it warm, and then place it at room temperature for 1 to 3 days to obtain sample H.
[0028] Furthermore, the process of step 9) is: placing the sample H on a flat-plate hot press at 150° C. to 165° C. for hot pressing and curing for 200 to 400 seconds to obtain a carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material.
[0029] The carbon nanotube grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material of the present invention is prepared by utilizing the preparation method of the carbon nanotube grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material.
[0030] The present invention has the following beneficial effects:
[0031] The carbon nanotube grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material and its preparation method described in the present invention introduce a silicon carbon nitrogen shell layer on the carbon fiber, and introduce high-density and uniformly distributed radial carbon nanotubes into the carbon fiber / phenolic resin composite material through the design of process steps. It should be noted that the maximum strength of the carbon fiber / phenolic resin composite material prepared by the present invention is 161.28MPa, and when the thickness is 0.4mm, the electromagnetic shielding effectiveness is 40.73dB. At the same time, the present invention realizes the high-density and uniform distribution of radial carbon nanotubes in the carbon fiber / phenolic resin composite material, and in the preparation process, the carbon fiber is not damaged. The reason for the improvement of strength is that the radial carbon nanotubes at the fiber / matrix interface increase the bonding force between the carbon fiber and the matrix. In addition, the radial carbon nanotubes penetrate deep into the interior of the matrix and can effectively hinder the matrix cracking caused by crack propagation under the action of external force. The reason for the improvement of electromagnetic shielding effectiveness is that when electromagnetic waves pass through the radial carbon nanotubes, multiple reflections and scattering will occur, causing a large amount of energy loss. In addition, the addition of radial carbon nanotubes improves the conductivity of the sample, increases the conductive loss, and improves the reflection efficiency of electromagnetic waves. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:
[0033] Figure 1 A scanning electron microscope photograph of the radial carbon nanotube-grafted silicon carbon nitrogen-carbon fiber prepared in Example 1;
[0034] Figure 2 This is another scanning electron microscope photo of the radial carbon nanotube-grafted silicon carbon nitride-carbon fiber prepared in Example 1.
[0035] Figure 3 This is another scanning electron microscope photo of the radial carbon nanotube-grafted silicon carbon nitride-carbon fiber prepared in Example 1.
[0036] Figure 4 A scanning electron microscope photograph of the silicon carbon nitride-carbon fiber prepared in step 4) of Example 4;
[0037] Figure 5 This is a scanning electron microscope photograph of the radial carbon nanotube-grafted silicon carbon nitride-carbon fiber prepared in step 6) of Example 4.
[0038] Figure 6 This is another scanning electron microscope photo of the silicon carbon nitride-carbon fiber prepared in step 4) of Example 4;
[0039] Figure 7 This is another scanning electron microscope photograph of the radial carbon nanotube-grafted silicon carbon nitride-carbon fiber prepared in step 6) of Example 4.
[0040] Figure 8 The tensile properties test diagram of the materials obtained in Example 1 and Example 4;
[0041] Fig. 9 These are electromagnetic shielding test diagrams of the materials obtained in Example 1 and Example 4. DETAILED DESCRIPTION
[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] In the description of the present invention, it should be understood that the terms “include” and “comprises” indicate the presence of described features, wholes, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, wholes, steps, operations, elements, components and / or collections thereof.
[0044] It should also be understood that the terms used in the present specification are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the present specification and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.
[0045] It should be further understood that the term "and / or" used in the present specification and the appended claims refers to any combination of one or more of the associated listed items and all possible combinations, and includes these combinations. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in the present invention generally indicates that the associated objects are in an "or" relationship.
[0046] It should be understood that, although the terms first, second, third, etc. may be used to describe preset ranges, etc. in the embodiments of the present invention, these preset ranges should not be limited to these terms. These terms are only used to distinguish preset ranges from each other. For example, without departing from the scope of the embodiments of the present invention, the first preset range may also be referred to as the second preset range, and similarly, the second preset range may also be referred to as the first preset range.
[0047] The word "if" as used herein may be interpreted as "at the time of" or "when" or "in response to determining" or "in response to detecting", depending on the context. Similarly, the phrases "if it is determined" or "if (stated condition or event) is detected" may be interpreted as "when it is determined" or "in response to determining" or "when detecting (stated condition or event)" or "in response to detecting (stated condition or event)", depending on the context.
[0048] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. The components of the embodiments of the present invention described and shown in the drawings here can usually be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0049] Various structural schematic diagrams of the embodiments disclosed in the present invention are shown in the accompanying drawings. These figures are not drawn to scale, and some details are magnified and some details may be omitted for the purpose of clear expression. The shapes of various regions and layers shown in the figures and the relative sizes and positional relationships therebetween are only exemplary, and may deviate in practice due to manufacturing tolerances or technical limitations, and those skilled in the art may additionally design regions / layers with different shapes, sizes, and relative positions according to actual needs.
[0050] The method for preparing the carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material of the present invention comprises the following steps:
[0051] 1) Place the carbon fiber cloth in a chemical vapor deposition furnace, heat it to 1000°C to 1100°C, use natural gas as the carbon source gas with a flow rate of 0.8L / min to 1L / min, and use argon as the protective gas with a flow rate of 2.0L / min to 2.4L / min, keep it warm for 2 to 4 hours, and obtain sample A.
[0052] 2) The polysilazane and acetone are uniformly mixed to obtain a solution B, wherein the mass ratio of the polysilazane to the acetone is 1:4 to 1:6.
[0053] 3) Sample A is immersed in solution B for 5 to 10 minutes, and then placed at room temperature for 24 to 48 hours to obtain sample C.
[0054] 4) Place sample C in a tubular heat treatment furnace, heat it to 150°C to 300°C and keep it warm for 2 to 3 hours, then heat it to 800°C to 950°C and keep it warm for 2 to 3 hours, wherein the heating rate is 2.5°C / min to 5°C / min. After the temperature in the tubular heat treatment furnace cools to room temperature, take out the sample to obtain sample D.
[0055] 5) Evenly mix ferrocene, anhydrous ethanol and ferrocene to obtain solution E, wherein the mass ratio of ferrocene to anhydrous ethanol is 1:80-1:100, and the mass ratio of ferrocene to ethylenediamine is 1:15-1:18.
[0056] 6) Place sample D in a tubular chemical vapor deposition furnace, heat it to 800°C to 900°C, inject solution E into the tubular chemical vapor deposition furnace at a rate of 5L / min to 15ml / h for 10 to 30 minutes, and take out the sample after the temperature in the tubular chemical vapor deposition furnace cools to room temperature to obtain sample F.
[0057] 7) The phenolic resin powder and anhydrous ethanol are uniformly mixed to obtain a solution G, wherein the mass ratio of the phenolic resin powder to the anhydrous ethanol is 1:3 to 1:2.
[0058] 8) Sample F is soaked in solution G for 1 to 3 days, taken out and placed in an oven, kept warm at 70 degrees Celsius for 10 minutes, and then placed at room temperature for 1 to 3 days to obtain sample H.
[0059] 9) Place sample H on a flat hot press at 150° C. to 165° C. and heat press and cure for 200 to 400 seconds to obtain a carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material.
[0060] Embodiment 1
[0061] This embodiment includes the following steps:
[0062] 1) Place the carbon fiber cloth in a chemical vapor deposition furnace, raise the temperature to 1000° C., use natural gas as the carbon source gas with a flow rate of 0.8 L / min, and argon as the protective gas with a flow rate of 2.0 L / min. Keep the temperature for 4 hours to obtain sample A.
[0063] 2) uniformly mixing polysilazane and acetone to obtain solution B, wherein the mass ratio of polysilazane to acetone is 1:6.
[0064] 3) Sample A was immersed in solution B for 10 minutes and then placed at room temperature for 24 hours to obtain sample C.
[0065] 4) Place sample C in a tubular heat treatment furnace, heat it to 300°C and keep it for 2 hours, then heat it to 800°C and keep it for 3 hours, wherein the heating rate is 2.5°C / min. After the temperature in the tubular heat treatment furnace cools to room temperature, take out the sample to obtain sample D.
[0066] 5) Ferrocene, anhydrous ethanol and ferrocene are uniformly mixed to obtain solution E, wherein the mass ratio of ferrocene to anhydrous ethanol is 1:80, and the mass ratio of ferrocene to ethylenediamine is 1:15.
[0067] 6) Place sample D in a tubular chemical vapor deposition furnace, heat it to 800°C, inject solution E into the tubular chemical vapor deposition furnace at a rate of 5 ml / h for 30 minutes, and take out the sample after the temperature in the tubular chemical vapor deposition furnace cools to room temperature to obtain sample F.
[0068] 7) The phenolic resin powder and anhydrous ethanol are uniformly mixed to obtain a solution G, wherein the mass ratio of the phenolic resin powder to the anhydrous ethanol is 1:3.
[0069] 8) Sample F was immersed in solution G for 3 days, taken out and placed in an oven, kept at 70 degrees Celsius for 10 minutes, and then placed at room temperature for 3 days to obtain sample H.
[0070] 9) Sample H was placed on a flat-plate hot press at 165° C. and hot-pressed for 200 seconds to obtain a carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material.
[0071] Embodiment 2
[0072] This embodiment includes the following steps:
[0073] 1) Place the carbon fiber cloth in a chemical vapor deposition furnace, raise the temperature to 1100° C., use natural gas as the carbon source gas with a flow rate of 1 L / min, and argon as the protective gas with a flow rate of 2.4 L / min. Keep the temperature for 2 hours to obtain sample A.
[0074] 2) uniformly mixing polysilazane and acetone to obtain solution B, wherein the mass ratio of polysilazane to acetone is 1:4.
[0075] 3) Sample A was immersed in solution B for 10 minutes and then placed at room temperature for 48 hours to obtain sample C.
[0076] 4) Place sample C in a tubular heat treatment furnace, heat it to 300°C and keep it for 3 hours, then heat it to 950°C and keep it for 3 hours, wherein the heating rate is 5°C / min. After the temperature in the tubular heat treatment furnace cools to room temperature, take out the sample to obtain sample D.
[0077] 5) Ferrocene, anhydrous ethanol and ferrocene are uniformly mixed to obtain solution E, wherein the mass ratio of ferrocene to anhydrous ethanol is 1:80, and the mass ratio of ferrocene to ethylenediamine is 1:15.
[0078] 6) Place sample D in a tubular chemical vapor deposition furnace, heat it to 800°C, inject solution E into the tubular chemical vapor deposition furnace at a rate of 5 ml / h for 10 minutes, and take out the sample after the temperature in the tubular chemical vapor deposition furnace cools to room temperature to obtain sample F.
[0079] 7) The phenolic resin powder and anhydrous ethanol are uniformly mixed to obtain a solution G, wherein the mass ratio of the phenolic resin powder to the anhydrous ethanol is 1:3.
[0080] 8) Sample F was immersed in solution G for 1 day, taken out and placed in an oven, kept warm at 70°C for 10 minutes, and then placed at room temperature for 1 day to obtain sample H.
[0081] 9) Sample H was placed on a flat-plate hot press at 150° C. and hot-pressed for 200 seconds to obtain a carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material.
[0082] Embodiment 3
[0083] This embodiment includes the following steps:
[0084] 1) The carbon fiber cloth was placed in a chemical vapor deposition furnace, the temperature was raised to 1100° C., natural gas was used as the carbon source gas with a flow rate of 0.8 L / min, argon was used as the protective gas with a flow rate of 2.0 L / min, and the temperature was kept for 4 hours to obtain sample A.
[0085] 2) uniformly mixing polysilazane and acetone to obtain solution B, wherein the mass ratio of polysilazane to acetone is 1:4.
[0086] 3) Sample A was immersed in solution B for 5 minutes and then placed at room temperature for 48 hours to obtain sample C.
[0087] 4) Place sample C in a tubular heat treatment furnace, heat it to 150°C and keep it for 3 hours, then heat it to 800°C and keep it for 3 hours, wherein the heating rate is 2.5°C / min. After the temperature in the tubular heat treatment furnace cools to room temperature, take out the sample to obtain sample D.
[0088] 5) Evenly mix ferrocene, anhydrous ethanol and ferrocene to obtain solution E, wherein the mass ratio of ferrocene to anhydrous ethanol is 1:100, and the mass ratio of ferrocene to ethylenediamine is 1:15.
[0089] 6) Place sample D in a tubular chemical vapor deposition furnace, heat it to 900°C, inject solution E into the tubular chemical vapor deposition furnace at a rate of 5 ml / h for 30 minutes, and take out the sample after the temperature in the tubular chemical vapor deposition furnace cools to room temperature to obtain sample F.
[0090] 7) The phenolic resin powder and anhydrous ethanol are uniformly mixed to obtain a solution G, wherein the mass ratio of the phenolic resin powder to the anhydrous ethanol is 1:3.
[0091] 8) Sample F was immersed in solution G for 3 days, taken out and placed in an oven, kept warm at 70°C for 10 minutes, and then placed at room temperature for 1 day to obtain sample H.
[0092] 9) Sample H was placed on a flat-plate hot press at 165° C. and hot-pressed for 200 seconds to obtain a carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material.
[0093] Embodiment 4
[0094] This embodiment includes the following steps:
[0095] 1) Place the carbon fiber cloth in a chemical vapor deposition furnace, raise the temperature to 1000° C., use argon as a protective gas with a flow rate of 2.0 to 2.4 L / min, and keep the temperature for 2 hours to obtain sample A.
[0096] 2) Polysilazane and acetone are uniformly mixed in a mass ratio of 1:4 to obtain solution B.
[0097] 3) Sample A was immersed in solution B for 10 minutes and then placed at room temperature for 48 hours to obtain sample C.
[0098] 4) Place sample C in a tubular heat treatment furnace, heat it to 150°C and keep it for 2 hours, then heat it to 950°C and keep it for 2 hours, with a heating rate of 5°C / min. After the temperature in the furnace cools to room temperature, take out the sample to obtain sample D.
[0099] 5) Evenly mix ferrocene, anhydrous ethanol and ferrocene, wherein the mass ratio of ferrocene to anhydrous ethanol is 1:80, and the mass ratio of ferrocene to ethylenediamine is 1:18, and stir evenly to obtain solution E.
[0100] 6) Place sample D in a tubular chemical vapor deposition furnace, heat it to 800°C, inject solution E into the tubular chemical vapor deposition furnace at a rate of 15 ml / h for 10 minutes, and take out the sample after the temperature in the furnace cools to room temperature to obtain sample F.
[0101] 7) The phenolic resin powder and anhydrous ethanol were uniformly mixed in a mass ratio of 1:2, and stirred to obtain a solution G.
[0102] 8) Sample F was immersed in solution G for 1 day, taken out and placed in an oven, kept warm at 70°C for 10 minutes, and placed at room temperature for 3 days to obtain sample H.
[0103] 9) Sample H was placed on a flat-plate hot press at 150° C. and hot-pressed for 200 seconds to obtain a carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material.
[0104] In the fourth embodiment, since the pyrolytic carbon shell layer is not deposited in step 3, cracks appear on the silicon carbon nitride core-shell on the surface of the carbon fiber, and thus radially high-density and uniformly distributed carbon nanotubes cannot be obtained. The material strength is only 82 MPa, and the average electromagnetic shielding effectiveness in the X-band is only 16.19 dB.
[0105] refer to Figure 8 and Fig. 9 If the requirement of depositing pyrolytic carbon is not met in step 1), the silicon carbon nitrogen core-shell on the surface of the carbon fiber will crack due to the large difference in elastic modulus between silicon carbon nitrogen and carbon fiber, and thus high-density and uniformly distributed carbon nanotubes cannot be obtained. If the solution ratio requirement of step 2) is not met, the silicon carbon nitrogen content in the carbon fiber will be too high, and cracking will occur during the heating and cooling process, and radially high-density and uniformly distributed carbon nanotubes cannot be obtained. By comparing the force-displacement curves of Example 1 and Example 4, it can be seen that the tensile strength of Example 1 is 96.34% higher than that of Example 4. This proves the reinforcing effect of high-density and uniformly distributed carbon nanotubes on carbon fiber / phenolic resin composites. By comparing the electromagnetic shielding effectiveness curves of Example 1 and Example 4, it can be seen that the average electromagnetic shielding effectiveness of Example 1 reaches 40.73dB, which is 151.73% higher than that of Example 4. This proves that high-density and uniformly distributed carbon nanotubes significantly improve the electromagnetic shielding capability of carbon fiber / phenolic resin composites.
[0106] Embodiment 5
[0107] This embodiment includes the following steps:
[0108] 1) Place the carbon fiber cloth in a chemical vapor deposition furnace, raise the temperature to 1000° C., use natural gas as the carbon source gas with a flow rate of 1 L / min; use argon as the protective gas with a flow rate of 2.0 L / min, and keep the temperature for 4 hours to obtain sample A.
[0109] 2) Polysilazane and acetone are uniformly mixed at a mass ratio of 4:1 to obtain solution B.
[0110] 3) Sample A was immersed in solution B for 5 minutes and then placed at room temperature for 48 hours to obtain sample C.
[0111] 4) Place sample C in a tubular heat treatment furnace, heat it to 150°C and keep it for 3 hours, then heat it to 800°C and keep it for 3 hours, with a heating rate of 2.5°C / min. After the temperature in the furnace cools to room temperature, take out the sample to obtain sample D.
[0112] 5) Evenly mix ferrocene, anhydrous ethanol and ferrocene, and stir to obtain solution E, wherein the mass ratio of ferrocene to anhydrous ethanol is 1:100, and the mass ratio of ferrocene to ethylenediamine is 1:15.
[0113] 6) Place sample D in a tubular chemical vapor deposition furnace, heat it to 900°C, inject solution E into the tubular chemical vapor deposition furnace at a rate of 5 ml / h for 30 minutes, and take out the sample after the temperature in the furnace cools to room temperature to obtain sample F.
[0114] 7) The phenolic resin powder and anhydrous ethanol are uniformly mixed in a mass ratio of 1:3, and stirred to obtain a solution G.
[0115] 8) Sample F was immersed in solution G for 3 days, taken out and placed in an oven, kept warm at 70°C for 10 minutes, and then placed at room temperature for 1 day to obtain sample H.
[0116] 9) Sample H was placed on a flat-plate hot press at 165° C. and hot-pressed for 200 seconds to obtain a carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material.
[0117] In this embodiment 5, since the solution ratio requirement in step 2) is not met during the preparation process, the silicon, carbon and nitrogen content in the carbon fiber is too high, cracking occurs during the heating and cooling process, and radially high-density and uniformly distributed carbon nanotubes cannot be obtained.
[0118] Embodiment 6
[0119] The method for preparing the carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material of the present invention comprises the following steps:
[0120] 1) Place the carbon fiber cloth in a chemical vapor deposition furnace, raise the temperature to 1000° C., use natural gas as the carbon source gas with a flow rate of 0.8 L / min, and argon as the protective gas with a flow rate of 2.0 L / min. Keep the temperature for 2 hours to obtain sample A.
[0121] 2) uniformly mixing polysilazane and acetone to obtain solution B, wherein the mass ratio of polysilazane to acetone is 1:4.
[0122] 3) Sample A was immersed in solution B for 5 minutes and then placed at room temperature for 24 hours to obtain sample C.
[0123] 4) Place sample C in a tubular heat treatment furnace, heat it to 150°C and keep it for 2 hours, then heat it to 800°C and keep it for 2 hours, wherein the heating rate is 2.5°C / min. After the temperature in the tubular heat treatment furnace cools to room temperature, take out the sample to obtain sample D.
[0124] 5) Ferrocene, anhydrous ethanol and ferrocene are uniformly mixed to obtain solution E, wherein the mass ratio of ferrocene to anhydrous ethanol is 1:80, and the mass ratio of ferrocene to ethylenediamine is 1:15.
[0125] 6) Place sample D in a tubular chemical vapor deposition furnace, heat it to 800°C, inject solution E into the tubular chemical vapor deposition furnace at a rate of 5 ml / h for 10 minutes, and take out the sample after the temperature in the tubular chemical vapor deposition furnace cools to room temperature to obtain sample F.
[0126] 7) The phenolic resin powder and anhydrous ethanol are uniformly mixed to obtain a solution G, wherein the mass ratio of the phenolic resin powder to the anhydrous ethanol is 1:3.
[0127] 8) Sample F was immersed in solution G for 1 day, taken out and placed in an oven, kept warm at 70°C for 10 minutes, and then placed at room temperature for 1 day to obtain sample H.
[0128] 9) Sample H was placed on a flat-plate hot press at 150° C. and hot-pressed for 200 seconds to obtain a carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material.
[0129] Embodiment 7
[0130] The method for preparing the carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material of the present invention comprises the following steps:
[0131] 1) Place the carbon fiber cloth in a chemical vapor deposition furnace, raise the temperature to 1100° C., use natural gas as the carbon source gas with a flow rate of 1 L / min, and argon as the protective gas with a flow rate of 2.4 L / min. Keep the temperature for 4 hours to obtain sample A.
[0132] 2) uniformly mixing polysilazane and acetone to obtain solution B, wherein the mass ratio of polysilazane to acetone is 1:6.
[0133] 3) Sample A was immersed in solution B for 10 minutes and then placed at room temperature for 48 hours to obtain sample C.
[0134] 4) Place sample C in a tubular heat treatment furnace, heat it to 300°C and keep it for 3 hours, then heat it to 950°C and keep it for 3 hours, wherein the heating rate is 5°C / min. After the temperature in the tubular heat treatment furnace cools to room temperature, take out the sample to obtain sample D.
[0135] 5) Evenly mix ferrocene, anhydrous ethanol and ferrocene to obtain solution E, wherein the mass ratio of ferrocene to anhydrous ethanol is 1:100, and the mass ratio of ferrocene to ethylenediamine is 1:18.
[0136] 6) Place sample D in a tubular chemical vapor deposition furnace, heat it to 900°C, inject solution E into the tubular chemical vapor deposition furnace at a rate of 15 ml / h for 30 minutes, and take out the sample after the temperature in the tubular chemical vapor deposition furnace cools to room temperature to obtain sample F.
[0137] 7) The phenolic resin powder and anhydrous ethanol are uniformly mixed to obtain a solution G, wherein the mass ratio of the phenolic resin powder to the anhydrous ethanol is 1:2.
[0138] 8) Sample F was immersed in solution G for 3 days, taken out and placed in an oven, kept warm at 70°C for 10 minutes, and then placed at room temperature for 3 days to obtain sample H.
[0139] 9) Sample H was placed on a flat-plate hot press at 165° C. and hot-pressed for 400 seconds to obtain a carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material.
[0140] Embodiment 8
[0141] The method for preparing the carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material of the present invention comprises the following steps:
[0142] 1) Place the carbon fiber cloth in a chemical vapor deposition furnace, raise the temperature to 1050° C., use natural gas as the carbon source gas with a flow rate of 0.9 L / min, and argon as the protective gas with a flow rate of 2.2 L / min. Keep the temperature for 3 hours to obtain sample A.
[0143] 2) uniformly mixing polysilazane and acetone to obtain solution B, wherein the mass ratio of polysilazane to acetone is 1:5.
[0144] 3) Sample A was immersed in solution B for 7.5 minutes and then placed at room temperature for 26 hours to obtain sample C.
[0145] 4) Place sample C in a tubular heat treatment furnace, heat it to 220°C and keep it for 2.5 hours, then heat it to 870°C and keep it for 2.5 hours, wherein the heating rate is 3.5°C / min. After the temperature in the tubular heat treatment furnace cools to room temperature, take out the sample to obtain sample D.
[0146] 5) Evenly mix ferrocene, anhydrous ethanol and ferrocene to obtain solution E, wherein the mass ratio of ferrocene to anhydrous ethanol is 1:90, and the mass ratio of ferrocene to ethylenediamine is 1:16.5.
[0147] 6) Place sample D in a tubular chemical vapor deposition furnace, heat it to 850°C, inject solution E into the tubular chemical vapor deposition furnace at a rate of 10 ml / h for 20 minutes, and take out the sample after the temperature in the tubular chemical vapor deposition furnace cools to room temperature to obtain sample F.
[0148] 7) The phenolic resin powder and anhydrous ethanol are uniformly mixed to obtain a solution G, wherein the mass ratio of the phenolic resin powder to the anhydrous ethanol is 1:2.5.
[0149] 8) Sample F was immersed in solution G for 2 days, taken out and placed in an oven, kept warm at 70°C for 10 minutes, and then placed at room temperature for 2 days to obtain sample H.
[0150] 9) Sample H was placed on a flat-plate hot press at 158° C. and hot-pressed for 300 seconds to obtain a carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material.
[0151] Embodiment 9
[0152] The method for preparing the carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material of the present invention comprises the following steps:
[0153] 1) Place the carbon fiber cloth in a chemical vapor deposition furnace, raise the temperature to 1040°C, use natural gas as the carbon source gas with a flow rate of 0.85 L / min, and argon as the protective gas with a flow rate of 2.1 L / min, and keep the temperature for 2.5 hours to obtain sample A.
[0154] 2) uniformly mixing polysilazane and acetone to obtain solution B, wherein the mass ratio of polysilazane to acetone is 1:4.5.
[0155] 3) Sample A was immersed in solution B for 6 minutes and then placed at room temperature for 25 hours to obtain sample C.
[0156] 4) Place sample C in a tubular heat treatment furnace, heat it to 180°C and keep it for 2.2 hours, then heat it to 850°C and keep it for 2.2 hours, wherein the heating rate is 2.8°C / min. After the temperature in the tubular heat treatment furnace cools to room temperature, take out the sample to obtain sample D.
[0157] 5) Evenly mix ferrocene, anhydrous ethanol and ferrocene to obtain solution E, wherein the mass ratio of ferrocene to anhydrous ethanol is 1:85, and the mass ratio of ferrocene to ethylenediamine is 1:16.
[0158] 6) Place sample D in a tubular chemical vapor deposition furnace, heat it to 820°C, inject solution E into the tubular chemical vapor deposition furnace at a rate of 8 ml / h for 15 minutes, and take out the sample after the temperature in the tubular chemical vapor deposition furnace cools to room temperature to obtain sample F.
[0159] 7) The phenolic resin powder and anhydrous ethanol are uniformly mixed to obtain a solution G, wherein the mass ratio of the phenolic resin powder to the anhydrous ethanol is 1:2.2.
[0160] 8) Sample F was immersed in solution G for 1.5 days, taken out and placed in an oven, kept warm at 70°C for 10 minutes, and then placed at room temperature for 1.5 days to obtain sample H.
[0161] 9) Sample H was placed on a flat-plate hot press at 155° C. and hot-pressed for 250 seconds to obtain a carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material.
[0162] Embodiment 10
[0163] The method for preparing the carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material of the present invention comprises the following steps:
[0164] 1) Place the carbon fiber cloth in a chemical vapor deposition furnace, raise the temperature to 1020° C., use natural gas as the carbon source gas with a flow rate of 0.82 L / min, and argon as the protective gas with a flow rate of 2.1 L / min. Keep the temperature for 2.5 hours to obtain sample A.
[0165] 2) uniformly mixing polysilazane and acetone to obtain solution B, wherein the mass ratio of polysilazane to acetone is 1:4.5.
[0166] 3) Sample A was immersed in solution B for 9 minutes and then placed at room temperature for 27 hours to obtain sample C.
[0167] 4) Place sample C in a tubular heat treatment furnace, heat it to 250°C and keep it for 2.8 hours, then heat it to 900°C and keep it for 2.8 hours, wherein the heating rate is 4.5°C / min. After the temperature in the tubular heat treatment furnace cools to room temperature, take out the sample to obtain sample D.
[0168] 5) Evenly mix ferrocene, anhydrous ethanol and ferrocene to obtain solution E, wherein the mass ratio of ferrocene to anhydrous ethanol is 1:95, and the mass ratio of ferrocene to ethylenediamine is 1:17.
[0169] 6) Place sample D in a tubular chemical vapor deposition furnace, heat it to 880°C, inject solution E into the tubular chemical vapor deposition furnace at a rate of 12 ml / h for 25 minutes, and take out the sample after the temperature in the tubular chemical vapor deposition furnace cools to room temperature to obtain sample F.
[0170] 7) The phenolic resin powder and anhydrous ethanol are uniformly mixed to obtain a solution G, wherein the mass ratio of the phenolic resin powder to the anhydrous ethanol is 1:2.8.
[0171] 8) Sample F was immersed in solution G for 2.8 days, taken out and placed in an oven, kept warm at 70 degrees Celsius for 10 minutes, and then placed at room temperature for 2.8 days to obtain sample H.
[0172] 9) Sample H was placed on a flat-plate hot press at 160° C. and hot-pressed for curing for 350 seconds to obtain a carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material.
[0173] Those skilled in the art will readily appreciate other embodiments of the present invention after considering the specification and disclosure of the invention. This application is intended to cover any variations, uses or adaptations of the present invention that follow the general principles of the present invention and include common knowledge or customary techniques in the art that are not disclosed by the present invention. The specification and examples are to be considered exemplary only, and the true scope and spirit of the present invention are indicated by the following claims.
[0174] It should be understood that the present invention is not limited to the exact construction that has been described above and shown in the drawings and that various modifications and changes may be made without departing from the scope thereof. The scope of the present invention is limited only by the appended claims.
[0175] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural changes in the specification made to the above embodiments based on the technical essence of the present invention still fall within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a carbon nanotube grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material, It is characterized in that The following steps are involved: A silicon carbon nitride shell layer is introduced on the surface of carbon fiber, and then radial carbon nanotubes are grown using a catalytic chemical deposition method to obtain a carbon nanotube-grafted silicon carbon nitride-carbon fiber / phenolic resin composite material.
2. The method for preparing the carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material according to claim 1, It is characterized in that The specific steps include: 1) placing the carbon fiber cloth in a chemical vapor deposition furnace, heating it, and then using natural gas as a carbon source gas and argon as a protective gas for heat preservation to obtain sample A; 2) uniformly mixing polysilazane and acetone to obtain solution B; 3) Immerse sample A in solution B and place it at room temperature to obtain sample C; 4) placing sample C in a tubular heat treatment furnace, heating it up and then keeping it warm, and taking out the sample after the temperature in the tubular heat treatment furnace cools down to room temperature to obtain sample D; 5) Evenly mix ferrocene, anhydrous ethanol and ferrocene to obtain solution E; 6) placing sample D in a tubular chemical vapor deposition furnace and heating it, injecting solution E into the tubular chemical vapor deposition furnace, and taking out the sample after the temperature in the tubular chemical vapor deposition furnace is cooled to room temperature, thereby obtaining sample F; 7) uniformly mixing phenolic resin powder and anhydrous ethanol to obtain solution G; 8) Soaking sample F in solution G, taking it out and drying it, and then leaving it at room temperature to obtain sample H; 9) The sample H is subjected to hot pressing and curing to obtain a carbon nanotube grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material.
3. The method for preparing the carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material according to claim 2, It is characterized in that The process of step 1) is: The carbon fiber cloth was placed in a chemical vapor deposition furnace, the temperature was raised to 1000°C to 1100°C, natural gas was used as the carbon source gas with a flow rate of 0.8L / min to 1L / min, argon was used as the protective gas with a flow rate of 2.0L / min to 2.4L / min, and the temperature was kept for 2 to 4 hours to obtain sample A.
4. The method for preparing the carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material according to claim 2, It is characterized in that In step 2), the mass ratio of polysilazane to acetone is 1:4 to 1:6; In step 7), the mass ratio of phenolic resin powder to anhydrous ethanol is 1:3 to 1:
2.
5. The method for preparing the carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material according to claim 2, It is characterized in that In step 5), the mass ratio of ferrocene to anhydrous ethanol is 1:80 to 1:100, and the mass ratio of ferrocene to ethylenediamine is 1:15 to 1:
18.
6. The method for preparing the carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material according to claim 2, It is characterized in that The process of step 4) is: place sample C in a tubular heat treatment furnace, heat it to 150°C~300°C and keep it warm for 2~3 hours, then heat it to 800°C~950°C and keep it warm for 2~3 hours, wherein the heating rate is 2.5°C / min~5°C / min, and take out the sample after the temperature in the tubular heat treatment furnace cools to room temperature to obtain sample D.
7. The method for preparing the carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material according to claim 2, It is characterized in that The process of step 6) is: place sample D in a tubular chemical vapor deposition furnace, heat it to 800°C to 900°C, inject solution E into the tubular chemical vapor deposition furnace at a rate of 5ml / h to 15ml / h, and the injection time is 10 to 30 minutes. After the temperature in the tubular chemical vapor deposition furnace cools to room temperature, take out the sample to obtain sample F.
8. The method for preparing the carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material according to claim 2, It is characterized in that The process of step 8) is: soak sample F in solution G for 1 to 3 days, take it out and place it in an oven, heat it up and then keep it warm, and then place it at room temperature for 1 to 3 days to obtain sample H.
9. The method for preparing the carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material according to claim 1, It is characterized in that The process of step 9) is: placing sample H on a flat-plate hot press at 150° C. to 165° C. for hot pressing and curing for 200 to 400 seconds to obtain a carbon nanotube-grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material.
10. A carbon nanotube grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material, It is characterized in that The composite material is prepared by the method for preparing the carbon nanotube grafted silicon carbon nitrogen-carbon fiber / phenolic resin composite material according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of ceramic matrix composite internal thread
CN112759404A
Preparation method of carbon fiber surface grafted MWCNT multi-scale reinforced resin-based friction material
CN114456537A
Silicon carbide nano scraper knife grafted carbon fiber, carbon fiber composite material and preparation method
CN117802777A
Boron-modified silazanes for synthesis of sibnc ceramics
US20150030856A1
Cited By
Preparation method of carbon-containing refractory material
CN120309319A