Chemical regeneration method and regenerated fiber of waste PET-PBT (Polyethylene Terephthalate-Polybutylene Terephthalate)

By using low-temperature homogeneous depolymerization technology and composite spinning processing, the problems of low depolymerization efficiency and poor product quality in the recycling of waste PET-PBT have been solved, realizing the production of high-efficiency, low-temperature depolymerization and high-value-added recycled fibers.

CN118996674AActive Publication Date: 2024-11-22DONGHUA UNIV

Patent Information

Application Number
CN202411112388.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-22
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

Existing chemical recycling technologies for waste PET-PBT are mostly based on high-temperature heterogeneous depolymerization, which has low depolymerization efficiency, serious 1,4-butanediol cyclization side reactions, resulting in a decline in the quality of recycled products, and long and costly process flow.

Method used

Using low-temperature homogeneous depolymerization technology, ethylene glycol and 1,4-butanediol are used as depolymerization agents to degrade PET-PBT into ethylene terephthalate and butylene terephthalate depolymerization solutions through low-temperature alcoholysis. High-value-added PET-PBT parallel composite elastic fibers are then produced through composite spinning.

Benefits of technology

It achieves efficient, low-temperature depolymerization, reduces the cyclization side reaction of 1,4-butanediol, improves the recovery rate and the quality of recycled products, and meets the performance requirements of virgin PET-PBT.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004992615780000051
    Figure BDA0004992615780000051
Patent Text Reader

Abstract

The invention relates to a chemical regeneration method of waste PET-PBT (Polyethylene Terephthalate-Polybutylene Terephthalate) and regenerated fiber. The regeneration method comprises the following steps: dissolving the waste PET-PBT at 170-190 DEG C through a solvent and a cosolvent; then respectively taking ethylene glycol and 1, 4-butanediol as depolymerization agents to react for 10-30 minutes at the temperature of 170-190 DEG C, so as to prepare a depolymerization solution taking ethylene glycol terephthalate or butylene terephthalate as a main body; the preparation method comprises the following steps: respectively carrying out decoloration, purification and drying processing on a depolymerization solution, then carrying out polymerization processing to prepare regenerated PET-PBT copolyester chips rich in PET or PBT, and carrying out composite spinning processing on the two copolyester chips to prepare a regenerated product of which the thermal performance meets the performance requirements of petroleum-based native PET-PBT elastic fibers. Compared with the prior art, closed-loop recovery and high-quality regeneration of the waste PET-PBT can be realized, the recovery rate and the recovery efficiency are high, side reactions such as cyclization of 1, 4-butanediol at high temperature can be effectively avoided, and the defects in the prior art are overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a chemical regeneration technology for waste PET-PBT, and in particular to a method for achieving low-temperature homogeneous depolymerization of a mixture of PET and PBT by dissolving the mixture, and regenerating the mixture into PET-PBT parallel composite elastic fibers with high added value. Background Art

[0002] PET-PBT textiles have the excellent properties of both PET and PBT and are widely used in the field of elastic textiles. However, PET-PBT textiles are a polymer material that is difficult to degrade in the natural environment, and the raw materials for their preparation are all from non-renewable petroleum. With the development of the PET-PBT textile industry, the treatment of its waste has also become an urgent problem to be solved. At present, the recycling of polyester in the market mainly focuses on PET recycling, while there is relatively little research on the recycling of PET-PBT.

[0003] At present, the methods for regenerating waste PET-PBT mainly include physical method and chemical method. The physical method can be divided into melting regeneration, mechanical crushing regeneration, etc. The mechanical properties and dyeing properties of the regenerated products are poor and need to be downgraded for use. Chemical regeneration can achieve high-value utilization of waste PET-PBT and is the main research direction in the textile field.

[0004] Patent CN 114805766A first melt-processes the waste PET-PBT mixture, then depolymerizes it with ethylene glycol / 1,4-butanediol, and transesterifies the obtained monomer with methanol to obtain dimethyl terephthalate, thus realizing the recycling of waste PET-PBT. The depolymerization reaction temperature is between 190 and 240°C, the reaction pressure is 101 to 201 kPa, and the residence time is 1 to 2 hours.

[0005] Patent CN 105088410A obtains recycled PET slices by melting and regenerating waste PET bottle flakes, and then modifies the recycled PET slices and extrudes them into granules through a twin-screw extruder, and then prepares PBT-modified recycled PET particles with PBT, and then melt-spins them to prepare PBT-modified recycled PET elastic yarns. The spinning temperature is 240℃~280℃, and the spinning speed is 1000~1500m / min.

[0006] In summary, the current chemical regeneration technology of waste PET-PBT is mostly based on the high-temperature heterogeneous depolymerization reaction of PBT / PET, with low depolymerization efficiency and recovery rate, and 1,4-butanediol will undergo side reactions such as cyclization during the high-temperature depolymerization process, reducing the quality of the regenerated product. In addition, the preparation of dimethyl terephthalate through an ester exchange reaction with methanol has a long process flow and high cost. Therefore, it is urgent to develop a low-temperature homogeneous depolymerization technology for waste PET-PBT and a direct polymerization technology for the depolymerization product to reduce / avoid the cyclization reaction of 1,4-butanediol during the reaction process, improve the recovery rate, depolymerization efficiency and the quality of the regenerated product, which has important scientific significance and practical value. Summary of the invention

[0007] In response to the above problems, the present application provides a chemical regeneration of waste PET-PBT and regenerated fibers, which adopts low-temperature homogeneous depolymerization technology and direct polymerization technology of depolymerization products to reduce / avoid the cyclization reaction of 1,4-butanediol during the reaction process, improve the recovery rate, depolymerization efficiency and quality of regenerated products, and has important scientific significance and practical value. The thermodynamic properties of the regenerated PET-PBT fibers prepared based on the process method of the present invention meet the performance requirements of petroleum-based virgin products.

[0008] The present application first provides a chemical regeneration method for waste PET-PBT, comprising the following steps:

[0009] The first step: add 100 parts of waste PET-PBT, 100-600 parts of solvent, and 50-400 parts of co-solvent into a high-pressure reactor, heat to 170-190°C, and treat for 10-30 minutes at a stirring speed of 15-50r / min. Then add 50-400 parts of ethylene glycol and 0.5-5 parts of the first catalyst, continue to react for 10-30 minutes, and obtain a first crude depolymerization liquid. The first crude depolymerization liquid is decolorized, purified, and dried to obtain a first refined depolymer. That is, the mass ratio of waste PET-PBT, solvent, co-solvent, ethylene glycol, and first catalyst is 100:100-600:50-400:0.5-5:50-400:0.5-5.

[0010] Step 2: 100 parts of the first refined depolymer and 0.5 parts of the second catalyst are placed in a high-pressure reactor to obtain the first recycled PET-PBT copolyester chips through polymerization, that is, the mass ratio of the first refined depolymer to the second catalyst is 100:0.5.

[0011] Step 3: Add 100 parts of waste PET-PBT, 100-600 parts of solvent, and 50-400 parts of co-solvent into a high-pressure reactor, heat to 170-190°C, and treat for 10-30 minutes at a stirring speed of 15-50r / min. Then add 50-400 parts of 1,4-butanediol and 0.5-5 parts of the first catalyst, continue to react for 10-30 minutes, and obtain a second crude depolymerization liquid. The obtained second crude depolymerization liquid is decolorized and purified to obtain a second refined depolymer. That is, the mass ratio of PET-PBT, solvent, co-solvent, ethylene glycol, and the first catalyst is 100:100-600:50-400:0.5-5:50-400:0.5-5.

[0012] Step 4: 100 parts of the second refined depolymer obtained in step 3 and 0.5 parts of the second catalyst are placed in a high pressure reactor to obtain the second recycled PBT-PET copolyester chips through polymerization, that is, the mass ratio of the second refined depolymer to the second catalyst is 100:0.5.

[0013] Step 5: placing the first recycled PET-PBT copolyester slice and the second recycled PBT-PET copolyester slice in the feed hopper of the parallel composite spinning machine respectively, and obtaining the recycled elastic fiber through composite spinning process.

[0014] The parts per unit mass in each of the above steps may not be the same.

[0015] Preferably, the waste PET-PBT is one or more of waste mixed fabrics, waste PET-PBT composite fibers, and PET and PBT mixed plastics.

[0016] Preferably, the solvent in the depolymerization step is one or more of dimethyl sulfoxide, N-methylpyrrolidone, aniline, and nitrobenzene.

[0017] Preferably, the co-solvent in the depolymerization step is one or more of acetonitrile, anisole and dichloromethane.

[0018] Preferably, the first catalyst in the depolymerization step is one or more of an ionic liquid, a deep eutectic solvent and 1,5,7-triazabicyclo[4.4.0]dec-5-ene.

[0019] Preferably, the ionic liquid is one or more of 1,3-dimethylimidazolium chloride, 1,3-dimethylimidazolium bromide, and 1,3-dimethylimidazolium acetate.

[0020] Preferably, the deep eutectic solvent is one or more of 1,3-dimethylurea / zinc acetate and choline chloride / urea.

[0021] Preferably, in the chemical regeneration of waste PET-PBT and its fiber, the first refined depolymer is a mixture of ethylene terephthalate, butylene terephthalate, and hydroxyethyl (hydroxybutyl) terephthalate, wherein the content of ethylene terephthalate is higher than 80%.

[0022] Preferably, the chemical regeneration of waste PET-PBT and its fiber are characterized in that the content of PET in the first regenerated PET-PBT copolyester chips is higher than 80wt%, and the intrinsic viscosity of the first regenerated PET-PBT copolyester chips is not higher than 0.6dl / g.

[0023] Preferably, the second catalyst described in PET-PBT is one or more of tetrabutyl titanate, isopropyl titanate, antimony trioxide, and antimony glycol.

[0024] Preferably, the second refined depolymer of PET-PBT is a mixture of ethylene terephthalate, butylene terephthalate and hydroxyethyl (hydroxybutyl) terephthalate, wherein the content of butylene terephthalate is higher than 80wt%.

[0025] Preferably, the content of PBT in the second recycled PBT-PET copolyester chips of PET-PBT is higher than 80wt%, and the intrinsic viscosity is not lower than 0.9dl / g.

[0026] Preferably, the regenerated elastic fiber of PET-PBT is a parallel composite, wherein the content of the first regenerated PET-PBT copolyester is 30wt% to 80wt%, and the content of the second regenerated PBT-PET copolyester is 70wt% to 20wt%.

[0027] Compared with the prior art, the beneficial effects of the present invention are:

[0028] 1) The present invention uses ethylene glycol and 1,4-butanediol as depolymerization agents, respectively, and degrades PET-PBT into a depolymerization liquid mainly composed of ethylene terephthalate and a depolymerization liquid mainly composed of butylene terephthalate through a low-temperature homogeneous depolymerization reaction. There is almost no side reaction such as cyclization of 1,4-butanediol during the depolymerization process, and the depolymerization speed is fast, the recovery rate is high, and the quality of the regenerated product is excellent, which makes up for the shortcomings of the prior art.

[0029] 2) The present invention uses depolymerization liquid containing ethylene terephthalate and butylene terephthalate as raw materials to prepare PET-PBT copolyester containing PET as the main component and PBT-PET copolyester containing PBT as the main component. Through composite spinning processing, parallel composite elastic fibers with high added value are prepared, realizing closed-loop recovery and high added value recycling of PET-PBT. DETAILED DESCRIPTION

[0030] On the whole, the technical scheme provides a chemical regeneration of waste PET-PBT and regenerated fibers. The present application realizes the low-temperature and efficient alcoholysis of waste PET-PBT under the action of solvents and co-solvents, and the depolymerization products of ethylene glycol and 1,4-butanediol are respectively decolorized, purified, dried and processed, and then directly polycondensed into PET-PBT copolyesters with different contents, which solves the problem of difficult separation of monomers after depolymerization of waste PET-PBT. The regenerated PET-PBT copolyester slices are melt-composite spun. The mechanical properties of the regenerated PET-PBT parallel composite fibers prepared by the process method of the present invention, such as breaking strength and elongation at break, meet the original requirements.

[0031] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0032] Any features such as preparation methods, materials, structures or composition ratios that are not clearly described in this technical solution shall be deemed as common technical features disclosed in the prior art.

[0033] Unless otherwise specified, the number of portions described in the present invention refers to the value under the condition of equal unit mass. The unit mass is the mass of each portion. If each portion is 1g, the unit mass is 1g / portion, and 100 portions are equal to 100g.

[0034] The test steps of the intrinsic viscosity in each embodiment of the present invention are as follows:

[0035] Dissolve 0.25±0.005g of sample in 96.00±0.2% concentrated sulfuric acid and measure its viscosity using an Ubbelohde viscometer at 25°C. For specific test principles and methods, see GBT 12006.1-2009. Its intrinsic viscosity is calculated using the following formula:

[0036]

[0037] Where, [η] is the intrinsic viscosity, η sp is the specific viscosity, η r is the relative viscosity, C is the sample concentration, and the unit is g / dl.

[0038] Example 1

[0039] In this embodiment, a chemical regeneration method for waste PET-PBT is described, and the specific steps are as follows:

[0040] Step 1: Add 1kg of waste PET-PBT, 1kg of dimethyl sulfoxide solvent, and 0.5kg of acetonitrile co-solvent into a 5L polymerization kettle, add the mixture into a high-pressure reactor, heat to 170°C, and treat for 10 minutes at a stirring speed of 15r / min. Then, add 0.5kg of ethylene glycol and 5g of 1,3-dimethylimidazole chloride catalyst, react for 10 minutes at a stirring speed of 100r / min, and obtain a depolymerization liquid 1, in which the BHET monomer content is 82.9%. The first crude depolymerization liquid is decolorized, purified, and dried to obtain a first refined depolymer.

[0041] Step 2: 0.84 kg of the first refined depolymerized product and 4.2 g of tetrabutyl titanate catalyst were placed in a high-pressure reactor, the temperature was gradually raised to 275°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the first recycled PET-PBT copolyester chips with an intrinsic viscosity of 0.55 dl / g, wherein the PET content was 82.9%.

[0042] Step 3: Add 1kg of waste PET-PBT, 1kg of dimethyl sulfoxide solvent, and 0.5kg of acetonitrile co-solvent into a 5L polymerization kettle, add it into the high-pressure reactor, heat it to 170°C, and treat it for 10 minutes at a stirring speed of 15r / min. Then add 0.5kg of 1,4-butanediol and 5g of 1,3-dimethylimidazole chloride catalyst, react for 10 minutes at a stirring speed of 100r / min, and obtain depolymerization liquid 2, in which the BHBT monomer content is 80.7%. The obtained second crude depolymerization liquid is decolorized, purified, and dried to obtain the second refined depolymer.

[0043] Step 4: 0.84 kg of the second refined depolymerized product and 4.2 g of tetrabutyl titanate catalyst were placed in a high pressure reactor, the temperature was gradually raised to 275°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the second recycled PBT-PET copolyester chips with an intrinsic viscosity of 0.95 dl / g, wherein the PBT content was 80.7%.

[0044] Step 5: Take the first recycled PET-PBT copolyester slice and the second recycled PBT-PET copolyester slice to carry out two-component composite spinning processing, wherein the spinning temperature of the first recycled PET-PBT copolyester slice is 280°C, and the spinning temperature of the second recycled PBT-PET copolyester slice is 265°C, to obtain recycled PET-PBT parallel composite fiber. The elongation at break is 25.8%, and the fiber strength is 2.56 cN / dtex.

[0045] Example 2

[0046] In this embodiment, a chemical regeneration method for waste PET-PBT is described, and the specific steps are as follows:

[0047] Step 1: Add 0.8kg of waste PET-PBT, 0.8kg of N-methylpyrrolidone solvent, and 0.8kg of acetonitrile co-solvent into a 5L polymerization kettle, add the mixture into a high-pressure reactor, heat to 175°C, and treat for 15 minutes at a stirring speed of 30r / min. Then add 0.8kg of ethylene glycol and 8g of 1,3-dimethylurea / zinc acetate catalyst, react for 15 minutes at a stirring speed of 100r / min, and obtain a depolymerization liquid 1, in which the BHET monomer content is 83.3%. The first crude depolymerization liquid is decolorized, purified, and dried to obtain a first refined depolymer.

[0048] Step 2: 0.8 kg of the first refined depolymerized product and 4 g of isopropyl titanate catalyst were placed in a high-pressure reactor, the temperature was gradually raised to 275°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the first recycled PET-PBT copolyester chips with an intrinsic viscosity of 0.57 dl / g, wherein the PET content was 83.3%.

[0049] Step 3: Add 0.8kg of waste PET-PBT, 0.8kg of N-methylpyrrolidone solvent, and 0.8kg of acetonitrile co-solvent into a 5L polymerization kettle, add the mixture into the autoclave, heat it to 175°C, and treat it for 15 minutes at a stirring speed of 30r / min. Then add 0.8kg of 1,4-butanediol and 8g of 1,3-dimethylurea / zinc acetate catalyst, and react for 15 minutes at a stirring speed of 100r / min to obtain depolymerization liquid 2, in which the BHBT monomer content is 81.2%. The obtained second crude depolymerization liquid is decolorized, purified, and dried to obtain the second refined depolymerization product.

[0050] Step 4: 0.8 kg of the second refined depolymerized product and 4 g of isopropyl titanate catalyst were placed in a high-pressure reactor, the temperature was gradually raised to 255°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the second recycled PBT-PET copolyester chips with an intrinsic viscosity of 0.91 dl / g, wherein the PBT content was 81.2%.

[0051] Step 5: Take the first recycled PET-PBT copolyester slice and the second recycled PBT-PET copolyester slice to carry out two-component composite spinning processing, wherein the spinning temperature of the first recycled PET-PBT copolyester slice is 280°C, and the spinning temperature of the second recycled PBT-PET copolyester slice is 265°C, to obtain recycled PET-PBT parallel composite fiber. The elongation at break is 26.2%, and the fiber strength is 2.51 cN / dtex.

[0052] Example 3

[0053] In this embodiment, a chemical regeneration method for waste PET-PBT is described, and the specific steps are as follows:

[0054] Step 1: Add 0.4kg of waste PET-PBT, 1.2kg of dimethyl sulfoxide solvent, and 1.2kg of acetonitrile co-solvent into a 5L polymerization kettle, add the mixture into a high-pressure reactor, heat to 180°C, and treat for 30 minutes at a stirring speed of 50r / min. Then add 1.2kg of ethylene glycol and 6g of choline chloride / urea catalyst, react for 10 minutes at a stirring speed of 100r / min, and obtain a depolymerization liquid 1, in which the BHET monomer content is 83.6%. The first crude depolymerization liquid is decolorized, purified, and dried to obtain a first refined depolymer.

[0055] Step 2: 0.4 kg of the first refined depolymerized product and 2 g of antimony trioxide catalyst were placed in a high-pressure reactor, the temperature was gradually raised to 275°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the first regenerated PET-PBT copolyester chips with an intrinsic viscosity of 0.58 dl / g, in which the PET content was 83.6%.

[0056] Step 3: Add 0.4kg of waste PET-PBT, 1.2kg of dimethyl sulfoxide solvent, and 1.2kg of acetonitrile co-solvent into a 5L polymerization kettle, add the mixture into the autoclave, heat it to 180°C, and treat it for 30min at a stirring speed of 50r / min. Then add 1.2kg of 1,4-butanediol and 6g of choline chloride / urea catalyst, and react for 10min at a stirring speed of 100r / min to obtain depolymerization liquid 2, in which the BHBT monomer content is 82.5%. The obtained second crude depolymerization liquid is decolorized, purified, and dried to obtain the second refined depolymer.

[0057] Step 4: 0.4 kg of the second refined depolymerized product and 2 g of antimony trioxide catalyst were placed in a high-pressure reactor, the temperature was gradually raised to 255°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the second recycled PBT-PET copolyester chips with an intrinsic viscosity of 1.12 dl / g, wherein the PBT content was 82.5%.

[0058] Step 5: Take the first recycled PET-PBT copolyester slice and the second recycled PBT-PET copolyester slice to carry out two-component composite spinning processing, wherein the spinning temperature of the first recycled PET-PBT copolyester slice is 280°C, and the spinning temperature of the second recycled PBT-PET copolyester slice is 265°C, to obtain recycled PET-PBT parallel composite fiber. The elongation at break is 26.4%, and the fiber strength is 2.59 cN / dtex.

[0059] Example 4

[0060] In this embodiment, a chemical regeneration method for waste PET-PBT is described, and the specific steps are as follows:

[0061] Step 1: Add 0.3kg of waste PET-PBT, 1.8kg of aniline solvent, and 1.2kg of anisole co-solvent into a 5L polymerization kettle, add the mixture into a high-pressure reactor, heat to 185°C, and treat for 30 minutes at a stirring speed of 50r / min. Then add 1.2kg of ethylene glycol and 15g of 1,5,7-triazabicyclo[4.4.0]dec-5-ene catalyst, react for 30 minutes at a stirring speed of 100r / min, and obtain a depolymerization liquid 1, in which the BHET monomer content is 84.8%. The first crude depolymerization liquid is decolorized, purified, and dried to obtain a first refined depolymer.

[0062] Step 2: 0.32 kg of the first refined depolymerized product and 1.6 g of antimony trioxide catalyst were placed in a high-pressure reactor, the temperature was gradually raised to 275°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the first regenerated PET-PBT copolyester chips with an intrinsic viscosity of 0.59 dl / g, wherein the PET content was 84.8%.

[0063] Step 3: Add 0.3kg of waste PET-PBT, 1.8kg of aniline solvent, and 1.2kg of anisole co-solvent into a 5L polymerization kettle, add the mixture into the autoclave, heat to 185°C, and treat for 30 minutes at a stirring speed of 50r / min. Then add 1.2kg of 1,4-butanediol and 15g of 1,5,7-triazabicyclo[4.4.0]dec-5-ene catalyst, react for 30 minutes at a stirring speed of 100r / min, and obtain depolymerization liquid 2, in which the BHBT monomer content is 83.9%. The obtained second crude depolymerization liquid is decolorized, purified, and dried to obtain the second refined depolymerization product.

[0064] Step 4: 0.32 kg of the second refined depolymerized product and 1.6 g of antimony trioxide catalyst were placed in a high-pressure reactor, the temperature was gradually raised to 255°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the second recycled PBT-PET copolyester chips with an intrinsic viscosity of 1.09 dl / g, wherein the PBT content was 83.9%.

[0065] Step 5: Take the first recycled PET-PBT copolyester slice and the second recycled PBT-PET copolyester slice to carry out two-component composite spinning processing, wherein the spinning temperature of the first recycled PET-PBT copolyester slice is 280°C, and the spinning temperature of the second recycled PBT-PET copolyester slice is 265°C, to obtain recycled PET-PBT parallel composite fiber. The elongation at break is 26.7%, and the fiber strength is 2.61 cN / dtex.

[0066] Example 5

[0067] In this embodiment, a chemical regeneration method for waste PET-PBT is described, and the specific steps are as follows:

[0068] Step 1: Add 0.6 kg of waste PET-PBT, 3.6 kg of aniline solvent, and 0.6 kg of anisole co-solvent into a 5L polymerization kettle, add the mixture into a high-pressure reactor, heat to 190°C, and treat for 30 minutes at a stirring speed of 40 r / min. Then add 0.6 kg of ethylene glycol and 6 g of 1,3-dimethylimidazolium bromide catalyst, react for 10 minutes at a stirring speed of 100 r / min, and obtain a depolymerization liquid 1, in which the BHET monomer content is 83.2%. The first crude depolymerization liquid is decolorized, purified, and dried to obtain a first refined depolymer.

[0069] Step 2: 0.6 kg of the first refined depolymerized product and 3 g of antimony trioxide catalyst were placed in a high-pressure reactor, the temperature was gradually raised to 275°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the first regenerated PET-PBT copolyester chips with an intrinsic viscosity of 0.52 dl / g, wherein the PET content was 83.2%.

[0070] Step 3: Add 0.6kg of waste PET-PBT, 3.6kg of aniline solvent, and 0.6kg of anisole co-solvent into a 5L polymerization kettle, add the mixture into the autoclave, heat to 190°C, and treat for 30min at a stirring speed of 40r / min. Then add 0.6kg of 1,4-butanediol and 6g of 1,3-dimethylimidazolium bromide catalyst, react for 10min at a stirring speed of 100r / min, and obtain depolymerization liquid 2, in which the BHBT monomer content is 82.6%. The obtained second crude depolymerization liquid is decolorized, purified, and dried to obtain the second refined depolymerization product.

[0071] Step 4: 0.6 kg of the second refined depolymerized product and 3 g of antimony trioxide catalyst were placed in a high-pressure reactor, the temperature was gradually raised to 255°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the second recycled PBT-PET copolyester chips with an intrinsic viscosity of 0.99 dl / g, wherein the PBT content was 82.6%.

[0072] Step 5: Take the first recycled PET-PBT copolyester slice and the second recycled PBT-PET copolyester slice to carry out two-component composite spinning processing, wherein the spinning temperature of the first recycled PET-PBT copolyester slice is 280°C, and the spinning temperature of the second recycled PBT-PET copolyester slice is 265°C, to obtain recycled PET-PBT parallel composite fiber. The elongation at break is 26.8%, and the fiber strength is 2.69 cN / dtex.

[0073] Example 6

[0074] In this embodiment, a chemical regeneration method for waste PET-PBT is described, and the specific steps are as follows:

[0075] Step 1: Add 0.5kg of waste PET-PBT, 2kg of aniline solvent, and 1kg of dichloromethane co-solvent into a 5L polymerization kettle, add the mixture into a high-pressure reactor, heat to 170°C, and treat for 20 minutes at a stirring speed of 30r / min. Then add 1kg of ethylene glycol and 0.5g of 1,3-dimethylurea / zinc acetate catalyst, react for 20 minutes at a stirring speed of 100r / min, and obtain a depolymerization liquid 1, in which the BHET monomer content is 84.6%. The first crude depolymerization liquid is decolorized, purified, and dried to obtain a first refined depolymer.

[0076] Step 2: 0.5 kg of the first refined depolymerized product and 2.5 g of the catalyst ethylene glycol antimony are placed in a high-pressure reactor, the temperature is gradually raised to 275°C, the pressure in the reactor is gradually reduced to below 50 Pa, and the reaction is carried out for 4 hours to perform polycondensation reaction to obtain the first recycled PET-PBT copolyester chips with an intrinsic viscosity of 0.58 dl / g, wherein the PET content is 84.6%.

[0077] Step 3: Add 0.5kg of waste PET-PBT, 2kg of aniline solvent, and 1kg of dichloromethane co-solvent into a 5L polymerization kettle, add the mixture into the autoclave, heat it to 170°C, and treat it for 20min at a stirring speed of 30r / min. Then add 1kg of 1,4-butanediol and 0.5g of 1,3-dimethylurea / zinc acetate catalyst, and react for 20min at a stirring speed of 100r / min to obtain depolymerization liquid 2, in which the BHBT monomer content is 80.5%. The obtained second crude depolymerization liquid is decolorized, purified, and dried to obtain the second refined depolymerization product.

[0078] Step 4: 0.5 kg of the second refined depolymerized product and 2.5 g of the catalyst ethylene glycol antimony were placed in a high-pressure reactor, the temperature was gradually raised to 255°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the second recycled PBT-PET copolyester chips with an intrinsic viscosity of 0.97 dl / g, wherein the PBT content was 80.5%.

[0079] Step 5: Take the first recycled PET-PBT copolyester slice and the second recycled PBT-PET copolyester slice to carry out two-component composite spinning processing, wherein the spinning temperature of the first recycled PET-PBT copolyester slice is 280°C, and the spinning temperature of the second recycled PBT-PET copolyester slice is 265°C, to obtain recycled PET-PBT parallel composite fiber. The elongation at break is 26.3%, and the fiber strength is 2.55 cN / dtex.

[0080] Example 7

[0081] In this embodiment, a chemical regeneration method for waste PET-PBT is described, and the specific steps are as follows:

[0082] Step 1: Add 0.7kg of waste PET-PBT, 2.1kg of aniline solvent, and 2.1kg of dichloromethane co-solvent into a 5L polymerization kettle, add the mixture into a high-pressure reactor, heat to 175°C, and treat for 15 minutes at a stirring speed of 50r / min. Then add 2.1kg of ethylene glycol and 3.5g of choline chloride / urea catalyst, react for 30 minutes at a stirring speed of 100r / min, and obtain a depolymerization liquid 1, in which the BHET monomer content is 84.3%. The first crude depolymerization liquid is decolorized, purified, and dried to obtain a first refined depolymer.

[0083] Step 2: 0.7 kg of the first refined depolymerized product and 3.5 g of the catalyst ethylene glycol antimony were placed in a high-pressure reactor, the temperature was gradually raised to 275°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the first regenerated PET-PBT copolyester chips with an intrinsic viscosity of 0.53 dl / g, wherein the PET content was 84.3%.

[0084] Step 3: Add 0.7kg of waste PET-PBT, 2.1kg of aniline solvent, and 2.1kg of dichloromethane co-solvent into a 5L polymerization kettle, add the mixture into the autoclave, heat it to 175°C, and treat it for 15min at a stirring speed of 50r / min. Then add 2.1kg of 1,4-butanediol and 3.5g of choline chloride / urea catalyst, and react for 30min at a stirring speed of 100r / min to obtain depolymerization liquid 2, in which the BHBT monomer content is 81.8%. The obtained second crude depolymerization liquid is decolorized, purified, and dried to obtain the second refined depolymer.

[0085] Step 4: 0.7 kg of the second refined depolymerized product and 3.5 g of the catalyst ethylene glycol antimony were placed in a high-pressure reactor, the temperature was gradually raised to 255°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the second recycled PBT-PET copolyester chips with an intrinsic viscosity of 0.96 dl / g, wherein the PBT content was 81.8%.

[0086] Step 5: Take the first recycled PET-PBT copolyester slice and the second recycled PBT-PET copolyester slice to carry out two-component composite spinning processing, wherein the spinning temperature of the first recycled PET-PBT copolyester slice is 280°C, and the spinning temperature of the second recycled PBT-PET copolyester slice is 265°C, to obtain recycled PET-PBT parallel composite fiber. The elongation at break is 27.1%, and the fiber strength is 2.65 cN / dtex.

[0087] Example 8

[0088] In this embodiment, a chemical regeneration method for waste PET-PBT is described, and the specific steps are as follows:

[0089] Step 1: Add 0.6kg of waste PET-PBT, 1.2kg of nitrobenzene solvent, and 1.2kg of acetonitrile co-solvent into a 5L polymerization kettle, add the mixture into a high-pressure reactor, heat to 180°C, and treat for 10 minutes at a stirring speed of 20r / min. Then, add 1.8kg of ethylene glycol and 3g of 1,3-dimethylimidazole chloride catalyst, and react for 30 minutes at a stirring speed of 100r / min to obtain a depolymerization liquid 1, in which the BHET monomer content is 85.2%. The first crude depolymerization liquid is decolorized, purified, and dried to obtain a first refined depolymer.

[0090] Step 2: 0.6 kg of the first refined depolymerized product and 3 g of the catalyst ethylene glycol antimony were placed in a high-pressure reactor, the temperature was gradually raised to 275°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the first regenerated PET-PBT copolyester chips with an intrinsic viscosity of 0.54 dl / g, wherein the PET content was 85.2%.

[0091] Step 3: Add 0.6kg of waste PET-PBT, 1.2kg of nitrobenzene solvent, and 1.2kg of acetonitrile co-solvent into a 5L polymerization kettle, add the mixture into the autoclave, heat to 180°C, and treat for 10min at a stirring speed of 20r / min. Then add 1.8kg of 1,4-butanediol and 3g of 1,3-dimethylimidazole chloride catalyst, react for 30min at a stirring speed of 100r / min, and obtain depolymerization liquid 2, in which the BHBT monomer content is 84.1%. The obtained second crude depolymerization liquid is decolorized, purified, and dried to obtain the second refined depolymerization product.

[0092] Step 4: 0.6 kg of the second refined depolymerized product and 3 g of the catalyst ethylene glycol antimony were placed in a high-pressure reactor, the temperature was gradually raised to 255°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the second regenerated PBT-PET copolyester chips with an intrinsic viscosity of 0.93 dl / g, wherein the PBT content was 84.1%.

[0093] Step 5: Take the first recycled PET-PBT copolyester slice and the second recycled PBT-PET copolyester slice to carry out two-component composite spinning processing, wherein the spinning temperature of the first recycled PET-PBT copolyester slice is 280°C, and the spinning temperature of the second recycled PBT-PET copolyester slice is 265°C, to obtain recycled PET-PBT parallel composite fiber. The elongation at break is 26.3%, and the fiber strength is 2.53 cN / dtex.

[0094] Example 9

[0095] In this embodiment, a chemical regeneration method for waste PET-PBT is described, and the specific steps are as follows:

[0096] Step 1: Add 0.4kg of waste PET-PBT, 0.4kg of N-methylpyrrolidone solvent, and 1.6kg of acetonitrile co-solvent into a 5L polymerization kettle, heat to 185°C, and treat for 20 minutes at a stirring speed of 30r / min. Then add 1.6kg of ethylene glycol and 1.2g of 1,5,7-triazabicyclo[4.4.0]dec-5-ene catalyst, react for 30 minutes at a stirring speed of 100r / min to obtain a depolymerization liquid 1, in which the BHET monomer content is 83.4%. The first crude depolymerization liquid obtained is decolorized, purified, and dried to obtain a first refined depolymer.

[0097] Step 2: 0.4 kg of the first refined depolymerized product and 2 g of tetrabutyl titanate catalyst were placed in a high-pressure reactor, the temperature was gradually raised to 275°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the first recycled PET-PBT copolyester chips with an intrinsic viscosity of 0.58 dl / g, wherein the PET content was 83.4%.

[0098] Step 3: Add 0.4kg of waste PET-PBT, 0.4kg of N-methylpyrrolidone solvent, and 1.6kg of acetonitrile co-solvent into a 5L polymerization kettle, add the mixture into the autoclave, heat it to 185°C, and treat it for 20min at a stirring speed of 30r / min. Then add 1.6kg of 1,4-butanediol and 1.2g of 1,5,7-triazabicyclo[4.4.0]dec-5-ene catalyst, and react for 30min at a stirring speed of 100r / min to obtain depolymerization liquid 2, in which the BHBT monomer content is 82.7%. The obtained second crude depolymerization liquid is decolorized, purified, and dried to obtain the second refined depolymerization product.

[0099] Step 4: 0.4 kg of the second refined depolymerized product and 2 g of tetrabutyl titanate catalyst were placed in a high-pressure reactor, the temperature was gradually raised to 255°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the second recycled PBT-PET copolyester chips with an intrinsic viscosity of 1.08 dl / g, wherein the PBT content was 82.7%.

[0100] Step 5: Take the first recycled PET-PBT copolyester slice and the second recycled PBT-PET copolyester slice to carry out two-component composite spinning processing, wherein the spinning temperature of the first recycled PET-PBT copolyester slice is 280°C, and the spinning temperature of the second recycled PBT-PET copolyester slice is 265°C, to obtain recycled PET-PBT parallel composite fiber. The elongation at break is 27.4%, and the fiber strength is 2.68 cN / dtex.

[0101] Example 10

[0102] In this embodiment, a chemical regeneration method for waste PET-PBT is described, and the specific steps are as follows:

[0103] Step 1: Add 0.8kg of waste PET-PBT, 0.8kg of dimethyl sulfoxide solvent, and 0.4kg of anisole co-solvent into a 5L polymerization kettle, add the mixture into a high-pressure reactor, heat to 185°C, and treat for 30 minutes at a stirring speed of 40r / min. Then add 3.2kg of ethylene glycol and 2g of choline chloride / urea catalyst, react for 20 minutes at a stirring speed of 100r / min, and obtain a depolymerization liquid 1, in which the BHET monomer content is 82.5%. The first crude depolymerization liquid is decolorized, purified, and dried to obtain a first refined depolymer.

[0104] Step 2: 0.8 kg of the first refined depolymerized product and 4 g of isopropyl titanate catalyst were placed in a high-pressure reactor, the temperature was gradually raised to 275°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the first recycled PET-PBT copolyester chips with an intrinsic viscosity of 0.59 dl / g, wherein the PET content was 82.5%.

[0105] Step 3: Add 0.8kg of waste PET-PBT, 0.8kg of dimethyl sulfoxide solvent, and 0.4kg of anisole co-solvent into a 5L polymerization kettle, add the mixture to the autoclave, heat to 185°C, and treat for 30 minutes at a stirring speed of 40r / min. Then add 3.2kg of 1,4-butanediol and 2g of choline chloride / urea catalyst, react for 20 minutes at a stirring speed of 100r / min, and obtain depolymerization liquid 2, in which the BHBT monomer content is 81.5%. The obtained second crude depolymerization liquid is decolorized, purified, and dried to obtain the second refined depolymer.

[0106] Step 4: 0.8 kg of the second refined depolymerized product and 4 g of isopropyl titanate catalyst were placed in a high-pressure reactor, the temperature was gradually raised to 255°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the second recycled PBT-PET copolyester chips with an intrinsic viscosity of 1.16 dl / g, wherein the PBT content was 81.5%.

[0107] Step 5: Take the first recycled PET-PBT copolyester slice and the second recycled PBT-PET copolyester slice to carry out two-component composite spinning processing, wherein the spinning temperature of the first recycled PET-PBT copolyester slice is 280°C, and the spinning temperature of the second recycled PBT-PET copolyester slice is 265°C, to obtain recycled PET-PBT parallel composite fiber. The elongation at break is 25.9%, and the fiber strength is 2.66 cN / dtex.

[0108] Embodiment 11

[0109] In this embodiment, a chemical regeneration method for waste PET-PBT is described, and the specific steps are as follows:

[0110] Step 1: Add 0.3kg of waste PET-PBT, 1.8kg of dimethyl sulfoxide solvent, and 1.2kg of dichloromethane co-solvent into a 5L polymerization kettle, add the mixture into a high-pressure reactor, heat to 190°C, and treat for 10 minutes at a stirring speed of 50r / min. Then, add 1.2kg of ethylene glycol and 1.5g of 1,3-dimethylimidazolium bromide catalyst, react for 10 minutes at a stirring speed of 100r / min, and obtain a depolymerization liquid 1, in which the BHET monomer content is 85.3%. The first crude depolymerization liquid is decolorized, purified, and dried to obtain a first refined depolymer.

[0111] Step 2: 0.3 kg of the first refined depolymerized product and 1.5 g of isopropyl titanate catalyst were placed in a high-pressure reactor, the temperature was gradually raised to 275°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the first recycled PET-PBT copolyester chips with an intrinsic viscosity of 0.51 dl / g, wherein the PET content was 85.3%.

[0112] Step 3: Add 0.3kg of waste PET-PBT, 1.8kg of dimethyl sulfoxide solvent, and 1.2kg of dichloromethane co-solvent into a 5L polymerization kettle, add the mixture into the autoclave, heat to 190°C, and treat for 10 minutes at a stirring speed of 50r / min. Then add 1.2kg of 1,4-butanediol and 1.5g of 1,3-dimethylimidazolium bromide catalyst, react for 10 minutes at a stirring speed of 100r / min, and obtain depolymerization liquid 2, in which the BHBT monomer content is 83.7%. The obtained second crude depolymerization liquid is decolorized, purified, and dried to obtain the second refined depolymer.

[0113] Step 4: 0.3 kg of the second refined depolymerized product and 1.5 g of isopropyl titanate catalyst were placed in a high pressure reactor, the temperature was gradually raised to 255°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the second recycled PBT-PET copolyester chips with an intrinsic viscosity of 0.98 dl / g, of which the PBT content was 83.7%.

[0114] Step 5: Take the first recycled PET-PBT copolyester slice and the second recycled PBT-PET copolyester slice to carry out two-component composite spinning processing, wherein the spinning temperature of the first recycled PET-PBT copolyester slice is 280°C, and the spinning temperature of the second recycled PBT-PET copolyester slice is 265°C, to obtain recycled PET-PBT parallel composite fiber. The elongation at break is 26.9%, and the fiber strength is 2.57 cN / dtex.

[0115] Example 12

[0116] In this embodiment, a chemical regeneration method for waste PET-PBT is described, and the specific steps are as follows:

[0117] Step 1: Add 0.5kg of waste PET-PBT, 0.5kg of N-methylpyrrolidone solvent, and 2kg of anisole co-solvent into a 5L polymerization kettle, add the mixture into a high-pressure reactor, heat to 170°C, and treat for 25 minutes at a stirring speed of 50r / min. Then add 2kg of ethylene glycol and 2.5g of 1,5,7-triazabicyclo[4.4.0]dec-5-ene catalyst, react for 25 minutes at a stirring speed of 100r / min, and obtain a depolymerization liquid 1, in which the BHET monomer content is 85.1%. The first crude depolymerization liquid is decolorized, purified, and dried to obtain a first refined depolymer.

[0118] Step 2: 0.5 kg of the first refined depolymerized product and 2.5 g of tetrabutyl titanate catalyst were placed in a high-pressure reactor, the temperature was gradually raised to 275°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the first recycled PET-PBT copolyester chips, with an intrinsic viscosity of 0.56 dl / g, of which the PET content was 85.1%.

[0119] Step 3: Add 0.5kg of waste PET-PBT, 0.5kg of N-methylpyrrolidone solvent, and 2kg of anisole co-solvent into a 5L polymerization kettle, add the mixture into the autoclave, heat to 170°C, and treat for 25min at a stirring speed of 50r / min. Then add 2kg of 1,4-butanediol and 2.5g of 1,5,7-triazabicyclo[4.4.0]dec-5-ene catalyst, react for 25min at a stirring speed of 100r / min, and obtain depolymerization liquid 2, in which the BHBT monomer content is 83.2%. The obtained second crude depolymerization liquid is decolorized, purified, and dried to obtain the second refined depolymerization product.

[0120] Step 4: 0.5 kg of the second refined depolymerized product and 2.5 g of tetrabutyl titanate catalyst were placed in a high pressure reactor, the temperature was gradually raised to 255°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the second recycled PBT-PET copolyester chips with an intrinsic viscosity of 0.93 dl / g, of which the PBT content was 83.2%.

[0121] Step 5: Take the first recycled PET-PBT copolyester slice and the second recycled PBT-PET copolyester slice to carry out two-component composite spinning processing, wherein the spinning temperature of the first recycled PET-PBT copolyester slice is 280°C, and the spinning temperature of the second recycled PBT-PET copolyester slice is 265°C, to obtain recycled PET-PBT parallel composite fiber. The elongation at break is 25.8%, and the fiber strength is 2.63 cN / dtex.

[0122] Comparative Example 1

[0123] A chemical regeneration method for waste PET-PBT in this comparative example, the specific steps are as follows:

[0124] Step 1: Add 1kg of waste PET-PBT, 2kg of ethylene glycol and 5g of zinc acetate catalyst into a 5L polymerization reactor, heat to 200°C and react at a stirring speed of 100r / min for 2h to obtain a depolymerization liquid 1, wherein the BHET monomer content is 78.9%. The first crude depolymerization liquid is decolorized, purified and dried to obtain a first refined depolymer.

[0125] Step 2: 1 kg of the first refined depolymerized product and 5 g of tetrabutyl titanate catalyst were placed in a high-pressure reactor, the temperature was gradually raised to 275°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the first recycled PET-PBT copolyester chips, with an intrinsic viscosity of 0.53 dl / g, of which the PET content was 78.9%.

[0126] Step 3: Add 1kg of waste PET-PBT, 2kg of 1,4-butanediol and 5g of zinc acetate catalyst into a 5L polymerization reactor, heat to 200°C and react at a stirring speed of 100r / min for 2h to obtain depolymerization liquid 2, in which the BHBT monomer content is 74.6%. The obtained second crude depolymerization liquid is decolorized, purified and dried to obtain the first refined depolymerization product.

[0127] Step 4: 0.5 kg of the second refined depolymerized product and 2.5 g of tetrabutyl titanate catalyst were placed in a high pressure reactor, the temperature was gradually raised to 255°C, the pressure in the reactor was gradually reduced to below 50 Pa, and the reaction was carried out for 4 hours to perform polycondensation reaction to obtain the second recycled PBT-PET copolyester chips with an intrinsic viscosity of 0.92 dl / g, of which the PBT content was 74.6%.

[0128] Step 5: Take the first recycled PET-PBT copolyester slice and the second recycled PBT-PET copolyester slice to carry out two-component composite spinning processing, wherein the spinning temperature of the first recycled PET-PBT copolyester slice is 280°C, and the spinning temperature of the second recycled PBT-PET copolyester slice is 265°C, to obtain recycled PET-PBT parallel composite fiber. The elongation at break is 25.2%, and the fiber strength is 2.49 cN / dtex.

[0129] Analysis of Comparative Example 1 and the Examples of the present invention shows that:

[0130] In Comparative Example 1, the depolymerization reaction of waste PET-PBT was carried out at 200°C, while in the embodiment of the present invention, the temperature range of the depolymerization reaction was 170°C to 190°C, and the embodiment of the present invention adopted a lower reaction temperature. The depolymerization reaction time in Comparative Example 1 was 2 hours, while the depolymerization reaction time in the embodiment of the present invention ranged from 10 minutes to 30 minutes, indicating that the embodiment of the present invention may have a faster reaction rate.

[0131] In Comparative Example 1, the BHET monomer recovery rate is 78.9%, and the BHBT monomer recovery rate is 74.6%. In the embodiments of the present invention, the BHET monomer recovery rate ranges from 82.5% to 85.3%, and the BHET monomer recovery rate ranges from 80.7% to 84.1%, indicating that the embodiments of the present invention have a higher monomer recovery rate.

[0132] The elongation at break of the recycled PET-PBT parallel composite fiber obtained in Comparative Example 1 is 25.2%, and the fiber strength is 2.49 cN / dtex. In the embodiment of the present invention, the elongation at break of the recycled PET-PBT parallel composite fiber ranges from 25.8% to 27.4%, and the fiber strength ranges from 2.51 cN / dtex to 2.69 cN / dtex. The strength and elongation at break of the recycled PET-PBT parallel composite fiber are more in line with the required range of the original PET-PBT parallel composite fiber.

[0133] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A chemical regeneration method for waste PET-PBT, characterized in that: The following steps are involved: Step 1: adding waste PET-PBT, solvent and co-solvent into a high-pressure reactor, heating to 170-190° C., treating for 10-30 min at a stirring speed of 15-50 r / min, then adding ethylene glycol and a first catalyst, continuing the reaction for 10-30 min to obtain a first crude depolymerization liquid, decolorizing, purifying and drying the obtained first crude depolymerization liquid to obtain a first refined depolymer, wherein the mass ratio of waste PET-PBT, solvent, co-solvent, ethylene glycol and the first catalyst is 100:100-600:50-400:0.5-5:50-400:0.5-5; Step 2: placing the first refined depolymer and the second catalyst obtained in step 1 in a high-pressure reactor, and obtaining a first recycled PET-PBT copolyester chip by polymerization, wherein the mass ratio of the first refined depolymer and the second catalyst is 100:0.5; Step 3: adding waste PET-PBT, solvent and co-solvent into a high-pressure reactor, heating to 170-190° C., treating for 10-30 min at a stirring speed of 15-50 r / min, then adding 1,4-butanediol and the first catalyst, continuing the reaction for 10-30 min to obtain a second crude depolymerization liquid, decolorizing and purifying the obtained second crude depolymerization liquid to obtain a second refined depolymer, wherein the mass ratio of PET-PBT, solvent, co-solvent, ethylene glycol and the first catalyst is 100:100-600:50-400:0.5-5:50-400:0.5-5; Step 4: placing the second refined depolymer and the second catalyst obtained in step 3 in a high-pressure reactor, and obtaining a second recycled PBT-PET copolyester chip by polymerization, wherein the mass ratio of the second refined depolymer and the second catalyst is 100:0.5; Step 5: placing the first recycled PET-PBT copolyester chips and the second recycled PBT-PET copolyester chips in the feed hopper of the parallel composite spinning machine respectively, and obtaining the recycled elastic fiber through composite spinning process.

2. The chemical regeneration method of waste PET-PBT according to claim 1, characterized in that: In step 1 and step 3, the waste PET-PBT described in PET-PBT is one or more of waste mixed fabrics, waste PET-PBT composite fibers, and mixed plastics of waste PET and PBT.

3. The chemical regeneration method of waste PET-PBT according to claim 1, characterized in that: In step 1 and step 3, the solvent is one or more of dimethyl sulfoxide, N-methylpyrrolidone, aniline, and nitrobenzene; The co-solvent is one or more of acetonitrile, anisole and dichloromethane.

4. The chemical regeneration method of waste PET-PBT according to claim 1, characterized in that: In step 1 and step 3, the first catalyst is one or more of an ionic liquid, a deep eutectic solvent and 1,5,7-triazabicyclo[4.4.0]dec-5-ene.

5. The chemical regeneration method of waste PET-PBT according to claim 4, characterized in that: The ionic liquid is one or more of 1,3-dimethylimidazolium chloride, 1,3-dimethylimidazolium bromide, and 1,3-dimethylimidazolium acetate; The deep eutectic solvent is one or more of 1,3-dimethylurea / zinc acetate and choline chloride / urea.

6. The chemical regeneration method of waste PET-PBT according to claim 1, characterized in that: In the steps 1 and 2, the first refined depolymer is a mixture of ethylene terephthalate, butylene terephthalate and hydroxyethyl (hydroxybutyl) terephthalate, wherein the content of ethylene terephthalate is higher than 80wt%.

7. The chemical regeneration method of waste PET-PBT according to claim 1, characterized in that: In step 2 and step 5, the content of PET in the first recycled PET-PBT copolyester chips is higher than 80wt%, and the intrinsic viscosity of the first recycled PET-PBT copolyester chips is not higher than 0.6dl / g.

8. The chemical regeneration method of waste PET-PBT according to claim 1, characterized in that: In step 2 and step 4, the second catalyst is one or more of tetrabutyl titanate, isopropyl titanate, antimony trioxide, and antimony glycol.

9. The chemical regeneration method of waste PET-PBT according to claim 1, characterized in that: In step 3 and step 4, the second refined depolymer is a mixture of butylene terephthalate, ethylene terephthalate, and hydroxyethyl (hydroxybutyl) terephthalate, wherein the content of butylene terephthalate is higher than 80wt%; In step 4 and step 5, the content of PBT in the second recycled PBT-PET copolyester chips is higher than 80wt%, and the intrinsic viscosity is not lower than 0.9dl / g.

10. A regenerated fiber prepared by the method according to any one of claims 1 to 9, characterized in that the regenerated elastic fiber is a parallel composite fiber, wherein: The content of the first recycled PET-PBT copolyester is 30 wt % to 80 wt %, and the content of the second recycled PBT-PET copolyester is 70 wt % to 20 wt %.

Citation Information

Patent Citations

  • Method for preparing PBT (Polybutylene Terephthalate) from PBT and waste PET (Polyethylene Terephthalate) polyester thereof or / and PET-PBT mixed polyester

    CN114805766A

  • Method for preparing polyester chips through chemical recycling of waste polyester fibers

    CN116284710A

  • Upgrading and regenerating method of waste polyester

    CN117820659A

  • Method for the depolymerization of a terephthalate polyester

    EP4273190A1

  • Method for producing polybutylene terephthalate

    JP2005089572A

Cited By

  • Preparation method of recycled polyester based on solvent azeotropic transesterification

    CN122483310A