Back contact battery, manufacturing method thereof and photovoltaic module

High-temperature diffusion is solved by first forming a first doped semiconductor layer with a high diffusion temperature during the production process of the back contact solar cell, and then forming a second doped semiconductor layer with a low diffusion temperature, and retaining the doped semiconductor layer at the junction. and the heat spot problem improve the quality and yield of the battery and achieve uniform leakage current.

CN119008723APending Publication Date: 2024-11-22SHANGRAO JINKO SOLAR NO 3 INTELLIGENT MANUFACTURING CO LTD +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411215183.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When the back contact solar cells form P and N regions, high temperature diffusion leads to low ion concentration in the N region, affecting the battery quality and yield, and hot spot problems are prone to occur under the reverse bias voltage.

Method used

During the production process of the back contact battery, a first doped semiconductor layer with a higher diffusion temperature is first formed, and then a second doped semiconductor layer with a lower diffusion temperature is formed to avoid the influence of high temperatures and retain the doped semiconductor layer at the junction. to form a leakage path, providing a conductive path under the reverse bias voltage.

Benefits of technology

The quality and yield of the back contact battery are improved, the heat spot problem is avoided, and the risk of heat accumulation is reduced through uniform leakage current.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008723A_ABST
    Figure CN119008723A_ABST
Patent Text Reader

Abstract

The invention relates to a back contact cell, a manufacturing method thereof and a photovoltaic module, on one hand, in the manufacturing process of the back contact cell, a first doped semiconductor layer with a higher diffusion temperature is formed firstly, and then a second doped semiconductor layer with a lower diffusion temperature is formed, so that the doped semiconductor layer which is formed firstly is prevented from being influenced by high diffusion temperature; secondary diffusion of doped ions in the doped semiconductor layer which is formed firstly is avoided, so that the formed back contact battery meets an expected design standard, and the quality and the yield of the back contact battery are improved; on the other hand, the second doped semiconductor layer at the junction of the first region and the second region is reserved, so that the first doped semiconductor layer and the second doped semiconductor layer can form connection at the junction of the first region and the second region, and an electric leakage path can be provided for the back contact battery in a reverse bias voltage state; and the hot spot problem can be effectively avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of photovoltaic power generation technology, and in particular to a back contact cell and a manufacturing method thereof, and a photovoltaic module. Background Art

[0002] The positive and negative electrodes of the back-contact solar cell are both arranged on the back of the battery. There is no grid line blocking the front of the battery, which reduces the shading loss on the front of the battery, can maximize the use of incident light on the front of the battery, and improve the battery conversion rate.

[0003] However, back-contact solar cells still have many shortcomings, which limit the development of back-contact solar cells. Summary of the invention

[0004] The following is a summary of the subject matter of the detailed description of the present disclosure. This summary is not intended to limit the scope of the claims.

[0005] In a first aspect, the present disclosure provides a method for manufacturing a back contact battery, comprising the following steps:

[0006] providing a substrate, the substrate having a first conductivity type;

[0007] forming a first tunneling layer, a first intrinsic semiconductor layer and a borosilicate glass layer in sequence on the back side of the substrate;

[0008] irradiating the borosilicate glass layer with a laser to dope the first intrinsic semiconductor layer to form a first doped semiconductor layer, wherein the first doped semiconductor layer has a second conductivity type;

[0009] Etching and removing the borosilicate glass layer, the first doped semiconductor layer, and the first tunneling layer outside the first area on the back side to expose the substrate in the second area;

[0010] A second tunneling layer, a second intrinsic semiconductor layer and a phosphosilicate glass layer are sequentially formed on the back side, wherein the second tunneling layer, the second intrinsic semiconductor layer and the phosphosilicate glass layer cover the substrate in the second region and the borosilicate glass layer in the first region;

[0011] irradiating the phosphosilicate glass layer with laser to dope the second intrinsic semiconductor layer to form a second doped semiconductor layer, wherein the second doped semiconductor layer has the first conductivity type;

[0012] At least a portion of the phosphosilicate glass layer, a portion of the second doped semiconductor layer and a portion of the second tunneling layer on the borosilicate glass layer are etched away, and the remaining second doped semiconductor layer is connected to the first doped semiconductor layer at the junction of the first region and the second region.

[0013] In one of the embodiments, the phosphosilicate glass layer, the second doped semiconductor layer, and the second tunneling layer in the first sub-region of the first region near the boundary are retained;

[0014] The second tunneling layer, the second doped semiconductor layer, and the phosphosilicate glass layer retained in the second region extend to the first sub-region and cover the borosilicate glass layer in the first sub-region.

[0015] In one embodiment, the width of the first sub-region is 10%-100% of the width of the first region.

[0016] In one embodiment, the first region and the second region are alternately arranged on the back side, and the phosphosilicate glass layer, the second doped semiconductor layer and the second tunneling layer of the first sub-regions of the plurality of first regions are reserved at intervals.

[0017] In one embodiment, after etching away the borosilicate glass layer, the first intrinsic semiconductor layer and the first tunneling layer outside the first area on the back side, the method further includes:

[0018] A pyramid structure is formed in the second region on the back side, and the height of the pyramid structure is 2 μm-5 μm.

[0019] In a second aspect, the present disclosure provides a back-contact battery, comprising:

[0020] A substrate, the substrate has a first conductivity type, and a back surface of the substrate has first regions and second regions that are alternately arranged;

[0021] A first tunneling layer, a first doped semiconductor layer and a borosilicate glass layer are sequentially stacked on a side of the first region away from the substrate, and the first doped semiconductor layer has a second conductivity type;

[0022] A second tunneling layer, a second doped semiconductor layer and a phosphosilicate glass layer are sequentially stacked on a side of the second region away from the substrate, the second doped semiconductor layer has a first conductivity type, wherein the first doped semiconductor layer is formed before the second doped semiconductor layer;

[0023] The first region extends parallel to the second region. Along the extension direction of the first region, the first doped semiconductor layer and the second doped semiconductor layer are connected at the junction of the first region and the second region. A second tunneling layer is provided between the first doped semiconductor layer and the second doped semiconductor layer.

[0024] In one embodiment, the first region includes a first sub-region near the junction, and the second tunneling layer, the second doped semiconductor layer and the phosphosilicate glass layer of the second region extend to the first sub-region and cover the borosilicate glass layer of the first sub-region.

[0025] In one embodiment, the width of the first sub-region is 10%-100% of the width of the first region;

[0026] And / or, the second region on the back side has a pyramid structure, and a height of the pyramid structure is 2 μm-5 μm.

[0027] In one embodiment, the first region and the second region are alternately arranged on the back side, a plurality of first regions are connected to the second region at intervals, and a phosphosilicate glass layer, a second doped semiconductor layer and a second tunneling layer are sequentially stacked on the side of the borosilicate glass layer of the first sub-region of the plurality of first regions away from the substrate.

[0028] In a third aspect, the present disclosure provides a photovoltaic module, including a back-contact cell manufactured by the method for manufacturing a back-contact cell according to the first aspect, or including a back-contact cell according to the second aspect.

[0029] The back contact cell and its manufacturing method and photovoltaic module disclosed in the present invention, on the one hand, in the manufacturing process of the back contact cell, a first doped semiconductor layer with a higher diffusion temperature is first formed, and then a second doped semiconductor layer with a lower diffusion temperature is formed, so as to avoid the high temperature of diffusion affecting the doped semiconductor layer formed earlier and avoid causing secondary diffusion of doped ions in the doped semiconductor layer formed earlier, so that the formed back contact cell meets the expected design standards and improves the quality and yield of the back contact cell; on the other hand, the second doped semiconductor layer is retained at the junction of the first region and the second region, so that the first doped semiconductor layer and the second doped semiconductor layer can be connected at the junction of the first region and the second region, which can provide a leakage path for the back contact cell to be in a reverse bias voltage state and can effectively avoid the hot spot problem. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the conventional technology, the drawings required for use in the embodiments or the conventional technology descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0031] Figure 1 is a process flow chart of a method for manufacturing a back contact battery provided in one embodiment;

[0032] Figure 2 It is a schematic diagram of a structure after a first tunneling layer, a first intrinsic semiconductor layer and a borosilicate glass layer are sequentially formed on the back side of a substrate provided in an embodiment;

[0033] Figure 3 It is a schematic diagram of a structure after the first intrinsic semiconductor layer is doped to form a first doped semiconductor layer provided in an embodiment;

[0034] Figure 4 It is a schematic diagram of a structure after removing the borosilicate glass layer, the first doped semiconductor layer and the first tunneling layer outside the first region provided in an embodiment;

[0035] Figure 5 It is a schematic diagram of a structure after a second tunneling layer, a second intrinsic semiconductor layer and a phosphosilicate glass layer are sequentially formed on the back side provided in an embodiment;

[0036] Figure 6 It is a schematic diagram of the structure after the second intrinsic semiconductor layer is doped to form the second doped semiconductor layer provided in one embodiment;

[0037] Figure 7 It is a schematic diagram of a structure after a portion of the phosphosilicate glass layer, a portion of the second doped semiconductor layer and a portion of the second tunneling layer on the borosilicate glass layer are removed by a small amount of etching provided in an embodiment;

[0038] Figure 8 A schematic diagram of a structure after texturing on the front side of a substrate provided in an embodiment;

[0039] Fig. 9 Schematic diagram of the structure of a back contact battery provided in one embodiment.

[0040] Description of reference numerals:

[0041] 10. Substrate; 11. First tunneling layer; 12. First intrinsic semiconductor layer; 13. Borosilicate glass layer; 14. First doped semiconductor layer; 15. Back passivation anti-reflection layer; 16. First electrode; 17. Second electrode; 21. Second tunneling layer; 22. Second intrinsic semiconductor layer; 23. Phosphosilicate glass layer; 24. Second doped semiconductor layer; 25. Front passivation anti-reflection layer; a1. First region; a11. First sub-region; a2. Second region; a3. Isolation region; 30. Isolation trench. DETAILED DESCRIPTION

[0042] In order to facilitate understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present application are given in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thorough and comprehensive.

[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0044] As described in the background technology, there are still many shortcomings in back-contact solar cells, which limits the development of back-contact solar cells. The inventors of this application have found that back-contact solar cells form alternating P and N regions on the back. The battery substrate used in the relevant technology is basically an N-type substrate. In the process of forming the P and N regions, the N region is usually doped first and then the P region. However, the temperature of ion diffusion in the P region is higher than the temperature of ion diffusion in the N region. The high temperature of the P region may cause the N region ions to diffuse again, resulting in the N region ion concentration being lower than expected, affecting the quality and yield of the back-contact battery.

[0045] In addition, the P region and N region of the back-contact solar cell are alternately arranged on the back of the cell. The back-contact solar cell performs photoelectric conversion when used. Under a higher reverse bias voltage, leakage may occur at local points of the back-contact solar cell. A larger leakage current passes through the local leakage point, and heat accumulates at the local leakage point, causing a greater risk of causing hot spots.

[0046] In view of this, the present application provides a back-contact battery and a manufacturing method thereof, and a photovoltaic module. On the one hand, in the manufacturing process of the back-contact battery, a first doped semiconductor layer with a higher diffusion temperature is formed first, and then a second doped semiconductor layer with a lower diffusion temperature is formed, so as to avoid the high temperature of the diffusion affecting the doped semiconductor layer formed earlier, and to avoid causing secondary diffusion of doped ions in the doped semiconductor layer formed earlier, so that the formed back-contact battery meets the expected design standards, and improves the quality and yield of the back-contact battery; on the other hand, the second doped semiconductor layer is retained at the junction of the first region and the second region, so that the first doped semiconductor layer and the second doped semiconductor layer can be connected at the junction of the first region and the second region, which can provide a leakage path for the back-contact battery to be in a reverse bias voltage state, and can effectively avoid the hot spot problem.

[0047] According to an exemplary embodiment, the present application provides a method for manufacturing a back contact battery, such as Figure 1 As shown, the method for making a back contact battery includes the following steps:

[0048] Step S10: providing a substrate 10, wherein the substrate 10 has a first conductivity type.

[0049] Reference Figure 2 As shown, the substrate 10 may be a silicon substrate 10, and the substrate 10 includes a front surface and a back surface that are oppositely disposed. In this embodiment, the first conductivity type is N type.

[0050] In some embodiments, not shown in the drawings of this embodiment, the back side of the substrate 10 is polished to remove the damaged layer on the back side of the substrate 10, and a pyramid structure is formed on the back side of the substrate 10. The base size of the pyramid structure is 15 μm-20 μm, and the reflectivity of the pyramid structure is 35%-45%.

[0051] Step S20 : ​​forming a first tunneling layer 11 , a first intrinsic semiconductor layer 12 and a borosilicate glass layer 13 in sequence on the back side of the substrate 10 .

[0052] Reference Figure 2 As shown, the substrate 10 can be oxidized by wet oxidation or thermal oxidation technology to form a first tunneling layer 11 on the back of the substrate 10. The thickness of the first tunneling layer 11 is controlled to be 1nm-5nm. Specifically, the first tunneling layer 11 is a silicon oxide layer.

[0053] The first intrinsic semiconductor layer 12 and the borosilicate glass layer 13 may be sequentially deposited on a side of the first tunneling layer 11 away from the substrate 10 by using an atomic layer deposition (ALD) process or a chemical vapor deposition (CVD) process.

[0054] The material of the first intrinsic semiconductor layer 12 includes polysilicon; the thickness of the first intrinsic semiconductor layer 12 is 100 nm-300 nm.

[0055] The thickness of the borosilicate glass layer 13 is 20 nm-80 nm.

[0056] Step S30 : irradiating the borosilicate glass layer 13 with laser to dope the first intrinsic semiconductor layer 12 to form a first doped semiconductor layer 14 , wherein the first doped semiconductor layer 14 has the second conductivity type.

[0057] Refer to 2. Figure 3 As shown, a laser may be used to irradiate the entire borosilicate glass layer 13 or selectively irradiate the borosilicate glass layer 13 in the first region a1. After the borosilicate glass layer 13 absorbs the energy of the laser, its temperature increases. The temperature of the borosilicate glass layer 13 increases to a first preset temperature. The boron ions in the borosilicate glass layer 13 diffuse into the first intrinsic semiconductor layer 12, and the first intrinsic semiconductor layer 12 is doped to form a first doped semiconductor layer 14. In this embodiment, the first doped semiconductor layer 14 has a P-type conductivity.

[0058] The doping concentration of boron ions in the first doped semiconductor layer 14 can be controlled by controlling the laser irradiation duration.

[0059] For example, the doping concentration of boron ions in the first doped semiconductor layer 14 is 1×10 19 atoms / cm 3 -10×10 19 atoms / cm 3 .

[0060] Step S40 : etching and removing the borosilicate glass layer 13 , the first doped semiconductor layer 14 and the first tunneling layer 11 outside the first area a1 on the back side to expose the substrate 10 in the second area a2 .

[0061] Reference Figure 4 As shown, a plurality of first regions a1 and a plurality of second regions a2 are defined at intervals on the back of the substrate 10, and the first regions a1 and the second regions a2 are alternately arranged. The borosilicate glass layer 13, the first doped semiconductor layer 14 and the first tunneling layer 11 outside the first regions a1 are removed by laser etching.

[0062] The area of ​​the second region a2 on the back side of the substrate 10 accounts for 40%-70%. For example, the area of ​​the second region a2 on the back side of the substrate 10 accounts for 40%, 50%, 60% or 70%.

[0063] Step S50: A second tunneling layer 21, a second intrinsic semiconductor layer 22 and a phosphosilicate glass layer 23 are sequentially formed on the back side, and the second tunneling layer 21, the second intrinsic semiconductor layer 22 and the phosphosilicate glass layer 23 cover the substrate 10 of the second area a2 and the borosilicate glass layer 13 of the first area a1.

[0064] Reference Figure 5 As shown, ALD or CVD can be used to sequentially deposit a second tunneling layer 21, a second intrinsic semiconductor layer 22 and a phosphosilicate glass layer 23 to cover the exposed back side of the substrate 10 and the borosilicate glass layer 13, the first doped semiconductor layer 14 and the first tunneling layer 11 in the first area a1.

[0065] The thickness of the second tunneling layer 21 is controlled to be 1 nm-5 nm. For example, the thickness of the second tunneling layer 21 may be 1 nm, 2 nm, 3 nm, 4 nm, or 5 nm. The second tunneling layer 21 is specifically a silicon oxide layer.

[0066] The material of the second intrinsic semiconductor layer 22 includes polysilicon, and the thickness of the second intrinsic semiconductor layer 22 is 100nm-300nm. The thickness of the phosphorus silicon glass layer 23 is 20nm-80nm.

[0067] Step S60 : irradiating the phosphosilicate glass layer 23 with laser to dope the second intrinsic semiconductor layer 22 to form a second doped semiconductor layer 24 , wherein the second doped semiconductor layer 24 has the first conductivity type.

[0068] Reference Figure 6As shown, the entire surface of the phosphosilicate glass layer 23 is irradiated with laser, and the temperature of the phosphosilicate glass layer 23 increases to a second preset temperature after absorbing the energy of the laser, wherein the second preset temperature is lower than the first preset temperature, and the phosphorus ions in the phosphosilicate glass layer 23 diffuse into the second intrinsic semiconductor layer 22, and dope the second intrinsic semiconductor layer 22 to form a second doped semiconductor layer 24. In this embodiment, the second doped semiconductor layer 24 has an N-type conductivity. In this way, the second preset temperature thermal diffusion process of the second intrinsic semiconductor layer 22 will not cause secondary diffusion of the borosilicate glass layer 13, and the doping concentration of the first semiconductor doping layer will not change.

[0069] The doping concentration of phosphorus ions in the second doped semiconductor layer 24 can be controlled by controlling the laser irradiation duration.

[0070] For example, the doping concentration of phosphorus ions in the second doped semiconductor layer 24 is 1×10 20 atoms / cm 3 -8×10atoms / cm 3 .

[0071] Step S70: At least a portion of the phosphosilicate glass layer 23, a portion of the second doped semiconductor layer 24 and a portion of the second tunneling layer 21 on the borosilicate glass layer 13 are etched away, and the remaining second doped semiconductor layer 24 is connected to the first doped semiconductor layer 14 at the junction of the first area a1 and the second area a2.

[0072] Reference Figure 7 As shown, laser selective etching is used to remove at least part of the phosphosilicate glass layer 23, part of the second doped semiconductor layer 24 and part of the second tunneling layer 21 on the first area a1, so that the second doped semiconductor layers 24 of multiple second areas a2 are disconnected, but the second doped semiconductor layer 24 at the junction of the first area a1 and the second area a2 is retained. At the junction of the first area a1 and the second area a2, the first doped semiconductor layer 14 and the second doped semiconductor layer 24 are physically connected through the second tunneling layer 21. The second tunneling layer 21 is relatively thin. When the back contact battery is in a reverse bias state, a smaller reverse bias current can tunnel through the second tunneling layer 21 to electrically connect the first doped semiconductor layer 14 and the second doped semiconductor layer 24, forming a leakage path at the junction of the first area a1 and the second area a2. The leakage current leaks evenly through the leakage path, avoiding leakage current leakage through local points to cause heat accumulation, thereby reducing the risk of hot spots.

[0073] The first region a1 extends parallel to the second region a2, and along the extension direction of the first region a1, the first doped semiconductor layer 14 and the second doped semiconductor layer 24 are connected at the junction of the first region a1 and the second region a2. In other words, one side surface of the first doped semiconductor layer 14 is connected to the entire side surface of the second doped semiconductor layer 24, which increases the connection area between the first doped semiconductor layer 14 and the second doped semiconductor layer 24, and can provide a larger leakage through hole for the battery in the reverse bias state. The leakage current leaks evenly through the leakage path formed by the connection surface of the first doped semiconductor layer 14 and the second doped semiconductor layer 24, so that the leakage current leaks evenly, avoiding the hot spot problem caused by high heat due to local leakage.

[0074] In one embodiment, referring to Figure 7 As shown, the phosphosilicate glass layer 23, the second doped semiconductor layer 24 and the second tunneling layer 21 of the first sub-region a11 near the junction of the first region a1 are retained; the second tunneling layer 21, the second doped semiconductor layer 24 and the phosphosilicate glass layer 23 retained in the second region a2 extend to the first sub-region a11 and cover the borosilicate glass layer 13 of the first sub-region a11.

[0075] In one embodiment, the width of the first sub-region a11 is 10%-100% of the width of the first region a1.

[0076] In some embodiments, the width of the first sub-region a11 is 10%-50% of the width of the first region a1, wherein the width direction is a direction perpendicular to the extension direction of the first region a1. For example, the width of the first sub-region a11 is 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50% of the width of the first region a1.

[0077] In one example, the width of the first sub-region a11 is 10% of the width of the first region a1. In another example, the width of the first sub-region a11 is 20% of the width of the first region a1. In yet another example, the width of the first sub-region a11 is 30% of the width of the first region a1.

[0078] In one embodiment, referring to Figure 7 , Figure 8 , Fig. 9 As shown, the first area a1 and the second area a2 are alternately arranged on the back side, and the phosphosilicate glass layer 23, the second doped semiconductor layer 24 and the second tunneling layer 21 of the first sub-area a11 of the first area a1 are reserved at intervals. In other words, the first areas a1 and the second areas a2 are connected at intervals.

[0079] It can be understood that, in addition to the first area a1 and the second area a2 , there is also an isolation area a3 on the back side of the substrate 10 , and the isolation area a3 is formed between the adjacent first area a1 and the second area a2 .

[0080] In this embodiment, along the direction in which the first area a1 and the second area a2 are alternately arranged, the isolation area a3 is disposed between the first area a1 and the second area a2. Adjacent first areas a1 and second areas a2 are connected, or adjacent first areas a1 and second areas a2 are separated by the isolation area a3.

[0081] Reference Figure 7 , Figure 8 As shown, in the process of etching away at least part of the phosphosilicate glass layer 23, part of the second doped semiconductor layer 24 and part of the second tunneling layer 21 on the borosilicate glass layer 13 in step S70, the isolation region a3 is etched away to form an isolation groove 30 in the isolation region a3, and at least part of the phosphosilicate glass layer 23, the second doped semiconductor layer 24 and the second tunneling layer 21 on the first region a1 are etched away. Only part of the phosphosilicate glass layer 23, the second doped semiconductor layer 24 and the second tunneling layer 21 on the first region a1 connected to the second region a2 is retained, and a plurality of leakage paths arranged at intervals are formed along the direction in which the first region a1 and the second region a2 are alternately arranged.

[0082] In some embodiments, along the direction in which the first areas a1 and the second areas a2 are alternately arranged, several first areas a1 among the multiple first areas a1 are connected to the second areas a2 on one side and are separated from the second areas a2 on the other side by the isolation area a3; several first areas a1 among the multiple first areas a1 are separated from the second areas a2 on both sides by the isolation area a3.

[0083] In one embodiment, after the step S40 is performed to etch away the borosilicate glass layer 13, the first intrinsic semiconductor layer 12 and the first tunneling layer 11 outside the first area a1 on the back side, Figure 4 As shown, it also includes: step S41: forming a pyramid structure in the second area a2 on the back side, the height of the pyramid structure is 2 μm-5 μm. In this way, the photoelectric conversion area on the back side can be further increased, and the photoelectric conversion efficiency of the battery can be improved.

[0084] The exposed back side of the substrate 10 may be polished or textured to form a pyramid structure. In one example, the pyramid structure is formed by texture, the texture depth is 2 μm-5 μm, and the texture reflectivity is 10%-12%. In another example, the pyramid structure is formed by polishing, the polishing depth is 2 μm-5 μm, and the base size of the pyramid structure is 10 μm-20 μm.

[0085] In some embodiments, after step S70, refer to Figure 8 As shown, the film layer formed on the front surface of the substrate 10 in steps S20-S70 is removed by etching to expose the front surface of the substrate 10, and the front surface of the substrate 10 is textured to form a pyramid structure.

[0086] Then, refer to Fig. 9 As shown, a front passivation anti-reflection layer 25 is deposited on the front side of the substrate 10, and a back passivation anti-reflection layer 15 is deposited on the back side of the substrate 10. The front passivation anti-reflection layer 25 may include a silicon oxide layer and a silicon nitride layer stacked in sequence; the back passivation anti-reflection layer 15 may include a silicon oxide layer and a silicon nitride layer stacked in sequence. The front passivation anti-reflection layer 25 and the back passivation anti-reflection layer 15 may be formed in the same process.

[0087] Next, refer to Fig. 9 As shown, a first electrode 16 and a second electrode 17 are formed on the back side of the substrate 10 by screen printing. The first electrode 16 is formed on the first area a1, and the first electrode 16 penetrates the back passivation anti-reflection layer 15 to contact and connect with the first doped semiconductor layer 14; the second electrode 17 is formed on the second area a2, and the second electrode 17 penetrates the back passivation anti-reflection layer 15 to contact and connect with the second doped semiconductor layer 24.

[0088] According to an exemplary embodiment, the present disclosure provides a back contact battery, referring to Fig. 9 As shown, the back contact cell includes a substrate 10, the substrate 10 has a first conductivity type, and the back side of the substrate 10 has first regions a1 and second regions a2 arranged alternately, wherein the area of ​​the second regions a2 on the back side of the substrate 10 accounts for 40%-70%. For example, the area of ​​the second regions a2 on the back side of the substrate 10 accounts for 40%, 50%, 60% or 70%. The back contact cell further includes a first tunneling layer 11, a first doped semiconductor layer 14 and a borosilicate glass layer 13 stacked in sequence on a side of the first region a1 away from the substrate 10, the first doped semiconductor layer 14 having a second conductivity type; a second tunneling layer 21, a second doped semiconductor layer 24 and a phosphosilicate glass layer 23 stacked in sequence on a side of the second region a2 away from the substrate 10, the second doped semiconductor layer 24 having a first conductivity type, wherein the first doped semiconductor layer 14 is formed before the second doped semiconductor layer 24; the first region a1 extends parallel to the second region a2, along the extension direction of the first region a1, the first doped semiconductor layer 14 and the second doped semiconductor layer 24 are connected at the junction of the first region a1 and the second region a2, and a second tunneling layer 21 is provided between the first doped semiconductor layer 14 and the second doped semiconductor layer 24. In this embodiment, the first conductivity type is N-type and the second conductivity type is P-type.

[0089] The thickness of the first tunneling layer 11 is 1 nm-5 nm, and the first tunneling layer 11 is specifically a silicon oxide layer. The material of the first doped semiconductor layer 14 includes polysilicon, and the doping concentration of boron ions in the first doped semiconductor layer 14 is 1×10 19 atoms / cm 3 -10×10 19 atoms / cm 3 The thickness of the first doped semiconductor layer 14 is 100 nm-300 nm. The thickness of the borosilicate glass layer 13 is 20 nm-80 nm.

[0090] The thickness of the second tunneling layer 21 is 1 nm-5 nm. For example, the thickness of the second tunneling layer 21 may be 1 nm, 2 nm, 3 nm, 4 nm, or 5 nm. The second tunneling layer 21 is specifically a silicon oxide layer.

[0091] The material of the second doped semiconductor layer 24 includes polycrystalline silicon, and the doping concentration of boron ions in the second doped semiconductor layer 24 is 1×10 20 atoms / cm 3 -8×10 20 atoms / cm 3 The thickness of the second doped semiconductor layer 24 is 100 nm-300 nm. The thickness of the phosphosilicate glass layer 23 is 20 nm-80 nm.

[0092] In the back contact battery of this embodiment, the first doped semiconductor layer 14 with a higher diffusion temperature is formed before the second doped semiconductor layer 24 with a lower diffusion temperature, so as to avoid the temperature of the second doped semiconductor layer 24 being diffused to form the second doped semiconductor layer 24 causing the borosilicate glass layer 13 to diffuse into the first doped semiconductor layer 14 again, thereby improving the product quality and yield rate of the back contact battery; and further optimize the battery design so that the first doped semiconductor layer 14 and the second doped semiconductor layer 24 are connected at the junction of the first area a1 and the second area a2, and a second tunneling layer 21 is provided between the first doped semiconductor layer 14 and the second doped semiconductor layer 24. The second tunneling layer 21 is relatively thin. When the back contact battery is in a reverse bias state, a smaller reverse bias current can tunnel through the second tunneling layer 21, so that the first doped semiconductor layer 14 and the second doped semiconductor layer 24 are electrically connected, and a leakage path is formed at the junction of the first area a1 and the second area a2. The leakage current leaks evenly through the leakage path, so as to avoid the leakage current leaking through local points to cause heat accumulation, thereby reducing the risk of hot spots.

[0093] Furthermore, the first region a1 of the present embodiment extends parallel to the second region a2, and along the extension direction of the first region a1, the first doped semiconductor layer 14 is connected to the second doped semiconductor layer 24 at the junction of the first region a1 and the second region a2. One side surface of the first doped semiconductor layer 14 is connected to the entire side surface of the second doped semiconductor layer 24, which increases the connection area between the first doped semiconductor layer 14 and the second doped semiconductor layer 24, and can provide a larger leakage path for the battery in the reverse bias state. The leakage current is uniformly leaked through the leakage path formed by the connection surface of the first doped semiconductor layer 14 and the second doped semiconductor layer 24, avoiding the hot spot problem caused by high heat due to local leakage.

[0094] In one embodiment, referring to Fig. 9 As shown, the first region a1 includes a first subregion a11 near the junction, and the second tunneling layer 21, the second doped semiconductor layer 24 and the phosphosilicate glass layer 23 of the second region a2 extend to the first subregion a11 and cover the borosilicate glass layer 13 of the first subregion a11.

[0095] In one embodiment, the width of the first sub-region a11 is 10%-100% of the width of the first region a1.

[0096] In some embodiments, the width of the first sub-region a11 is 10%-50% of the width of the first region a1, wherein the width direction is a direction perpendicular to the extension direction of the first region a1. For example, the width of the first sub-region a11 is 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50% of the width of the first region a1.

[0097] In one example, the width of the first sub-region a11 is 10% of the width of the first region a1. In another example, the width of the first sub-region a11 is 20% of the width of the first region a1. In yet another example, the width of the first sub-region a11 is 30% of the width of the first region a1.

[0098] In one embodiment, referring to Fig. 9 As shown, the second area a2 on the back has a pyramid structure, and the height of the pyramid structure is 2μm-5μm. In one example, the suede reflectivity of the pyramid structure of the second area a2 is 10%-12%. In another example, the base size of the pyramid structure of the second area a2 is 10μm-20μm.

[0099] In one of the embodiments, which is not shown in the drawings of this embodiment, the first area a1 on the back side also has a pyramid structure, the base size of the pyramid structure of the first area a1 is 15 μm-20 μm, and the reflectivity of the pyramid structure is 35%-45%.

[0100] In one embodiment, referring to Fig. 9 As shown, the first area a1 and the second area a2 are alternately arranged on the back side, and multiple first areas a1 are connected to the second areas a2 at intervals, and the borosilicate glass layer 13 of the first sub-areas a11 of the multiple first areas a1 is stacked in sequence on the side away from the substrate 10 with a phosphosilicate glass layer 23, a second doped semiconductor layer 24 and a second tunneling layer 21.

[0101] Understandable, refer to Fig. 9 As shown, in addition to the first area a1 and the second area a2 , there is an isolation area a3 on the back side of the substrate 10 . The isolation area a3 is formed between the adjacent first area a1 and the second area a2 .

[0102] In this embodiment, along the direction in which the first region a1 and the second region a2 are alternately arranged, the isolation region a3 is disposed between the first region a1 and the second region a2 at intervals. The adjacent first region a1 is connected to the second region a2, or the adjacent first region a1 and the second region a2 are separated by the isolation region a3. That is, along the direction in which the first region a1 and the second region a2 are alternately arranged, part of the first region a1 is connected to the second region a2, and the first doped semiconductor layer 14 of the connected first region a1 is in contact with the second doped semiconductor layer 24 of the second region a2, forming a plurality of leakage paths at intervals.

[0103] In some embodiments, along the direction in which the first areas a1 and the second areas a2 are alternately arranged, several first areas a1 among the multiple first areas a1 are connected to the second areas a2 on one side and are separated from the second areas a2 on the other side by the isolation area a3; several first areas a1 among the multiple first areas a1 are separated from the second areas a2 on both sides by the isolation area a3.

[0104] The first area a1 and the second area a2 are connected, and the phosphosilicate glass layer 23, the second doped semiconductor layer 24 and the second tunneling layer 21 of the second area a2 extend to the first area a1, covering the borosilicate glass layer 13 of the first sub-area a11 of the first area a1, thereby increasing the size of the leakage path, avoiding heat accumulation due to leakage at local points when the back contact battery is in a reverse bias state, and further reducing the risk of hot spots.

[0105] In one embodiment, referring to Fig. 9 As shown, the back contact cell further includes a front passivation anti-reflection layer 25, which covers the front side of the substrate 10; the front passivation anti-reflection layer 25 may include a silicon oxide layer and a silicon nitride layer stacked in sequence.

[0106] Reference Fig. 9As shown, the back contact cell also includes a back passivation anti-reflection layer 15, which covers the borosilicate glass layer 13 and the phosphosilicate glass layer 23 on the back side of the substrate 10; the back passivation anti-reflection layer 15 may include a silicon oxide layer and a silicon nitride layer stacked in sequence.

[0107] In one embodiment, referring to Fig. 9 As shown, the back-contact battery also includes a first electrode 16 and a second electrode 17. The first electrode 16 is arranged on a first area a1 on the back side, and the first electrode 16 penetrates the back passivation anti-reflection layer 15 and is in contact with the first doped semiconductor layer 14; the second electrode 17 is arranged on a second area a2 on the back side, and the second electrode 17 penetrates the back passivation anti-reflection layer 15 and is in contact with the second doped semiconductor layer 24.

[0108] In a third aspect, the present disclosure provides a photovoltaic module, including a back-contact cell manufactured by the method for manufacturing a back-contact cell according to the first aspect, or including a back-contact cell according to the second aspect.

[0109] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features of the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0110] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A method for manufacturing a back contact battery, characterized in that: The following steps are involved: providing a substrate having a first conductivity type; forming a first tunneling layer, a first intrinsic semiconductor layer and a borosilicate glass layer in sequence on the back side of the substrate; irradiating the borosilicate glass layer with a laser to dope the first intrinsic semiconductor layer to form a first doped semiconductor layer, wherein the first doped semiconductor layer has a second conductivity type; Etching and removing the borosilicate glass layer, the first doped semiconductor layer, and the first tunneling layer outside the first area of ​​the back surface to expose the substrate in the second area; Forming a second tunneling layer, a second intrinsic semiconductor layer and a phosphosilicate glass layer in sequence on the back side, wherein the second tunneling layer, the second intrinsic semiconductor layer and the phosphosilicate glass layer cover the substrate in the second area and the borosilicate glass layer in the first area; irradiating the phosphosilicate glass layer with a laser to dope the second intrinsic semiconductor layer to form a second doped semiconductor layer, wherein the second doped semiconductor layer has a first conductivity type; At least a portion of the phosphosilicate glass layer, a portion of the second doped semiconductor layer and a portion of the second tunneling layer on the borosilicate glass layer are etched away, and the remaining second doped semiconductor layer is connected to the first doped semiconductor layer at a boundary between the first region and the second region.

2. The method for manufacturing a back contact battery according to claim 1, characterized in that: retaining the phosphosilicate glass layer, the second doped semiconductor layer and the second tunneling layer in a first sub-region of the first region close to the junction; The second tunneling layer, the second doped semiconductor layer, and the phosphosilicate glass layer retained in the second region extend to the first sub-region and cover the borosilicate glass layer in the first sub-region.

3. The method for manufacturing a back contact battery according to claim 2, characterized in that: The width of the first sub-region is 10%-100% of the width of the first region.

4. The method for manufacturing a back contact battery according to claim 2, characterized in that: The first region and the second region are alternately arranged on the back side, and the phosphosilicate glass layer, the second doped semiconductor layer, and the second tunneling layer of the first sub-regions of the first region are reserved at intervals.

5. The method for manufacturing a back contact battery according to any one of claims 1 to 4, characterized in that: After etching away the borosilicate glass layer, the first intrinsic semiconductor layer and the first tunneling layer outside the first area of ​​the back side, the method further includes: A pyramid structure is formed in the second region on the back surface, and the height of the pyramid structure is 2 μm-5 μm.

6. A back contact battery, characterized in that: include: A substrate, the substrate having a first conductivity type, and a back surface of the substrate having first regions and second regions arranged alternately; A first tunneling layer, a first doped semiconductor layer and a borosilicate glass layer are sequentially stacked on a side of the first region away from the substrate, wherein the first doped semiconductor layer has a second conductivity type; A second tunneling layer, a second doped semiconductor layer and a phosphosilicate glass layer are sequentially stacked on a side of the second region away from the substrate, the second doped semiconductor layer has a first conductivity type, wherein the first doped semiconductor layer is formed before the second doped semiconductor layer; The first region extends parallel to the second region. Along the extension direction of the first region, the first doped semiconductor layer and the second doped semiconductor layer are connected at the junction of the first region and the second region. The second tunneling layer is provided between the first doped semiconductor layer and the second doped semiconductor layer.

7. The back contact cell according to claim 6, characterized in that: The first region includes a first sub-region close to the junction, and the second tunneling layer, the second doped semiconductor layer and the phosphosilicate glass layer of the second region extend to the first sub-region and cover the borosilicate glass layer of the first sub-region.

8. The back contact battery according to claim 7, characterized in that: The width of the first sub-region is 10%-100% of the width of the first region; And / or, the second region on the back side has a pyramid structure, and the height of the pyramid structure is 2 μm-5 μm.

9. The back contact cell according to claim 7, characterized in that: The first regions and the second regions are alternately arranged on the back side, a plurality of the first regions are connected to the second region at intervals, and the phosphosilicate glass layer, the second doped semiconductor layer and the second tunneling layer are sequentially stacked on the side of the borosilicate glass layer of the first sub-region of a plurality of the first regions away from the substrate.

10. A photovoltaic module, characterized in that: A back contact battery manufactured by the method for manufacturing a back contact battery as described in any one of claims 1 to 5, or a back contact battery as described in any one of claims 6 to 9.

Citation Information

Cited By

  • Preparation method of back contact TBC battery

    CN119744021A

  • A method of manufacturing a back contact tbc cell

    CN119744021B