Lithium-doped silicon-carbon composite material with high initial efficiency and preparation method of lithium-doped silicon-carbon composite material

By depositing lithium hydride and heteroatoms in porous carbon, forming a core-shell structure, and depositing amorphous carbon on the surface of the shell, the problem of low conductivity of silicon-carbon composite materials is solved, and the first efficiency and cycling performance of lithium-ion batteries are improved.

CN119008908APending Publication Date: 2024-11-22云南坤天新能源有限公司
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411202220.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing silicon-carbon composite materials have poor electronic conductivity and low first-time efficiency, making it difficult to meet the requirements of lithium-ion batteries for high energy density and fast charging performance.

Method used

High-first-efficiency lithium-doped silicon-carbon composite material using core-shell structures can enhance electron conductivity by depositing lithium hydride and heteroatoms in porous carbon, and depositing amorphous carbon on the surface of the shell to enhance the cladding integrity and reduce expansion .

Benefits of technology

It significantly improves the first-time efficiency and cycling performance of lithium-ion batteries, reduces the expansion rate of the material and powder conductivity, and improves the specific surface area and conductivity of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008908A_ABST
    Figure CN119008908A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion battery materials, and provides a high-first-efficiency lithium-doped silicon-carbon composite material and a preparation method thereof.The lithium-doped silicon-carbon composite material is of a core-shell structure composed of an inner core and an outer shell, the inner core is lithium-silicon-doped porous carbon, and the outer shell is heteroatom-doped amorphous carbon. According to the technical scheme, the problems of poor conductivity and low first efficiency of the silicon-carbon composite material in the prior art are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of silicon-carbon composite materials, and in particular to a high first efficiency lithium-doped silicon-carbon composite material and a preparation method thereof. Background Art

[0002] As the market's requirements for the energy density of lithium-ion batteries increase, the negative electrode materials used in lithium-ion batteries are required to have high energy density while also having improved fast charging performance. The new silicon-carbon material is a new type of negative electrode material with high specific capacity, high initial efficiency and low expansion. Although porous carbon has the advantages of large specific surface area and internal porosity, it also has some defects, resulting in poor electronic conductivity and low initial efficiency. Therefore, it is necessary to improve the electronic and ionic conductivity and initial efficiency of silicon-carbon materials and improve rate performance. Summary of the invention

[0003] The present invention provides a high first efficiency lithium-doped silicon-carbon composite material and a preparation method thereof, which solves the problems of poor conductivity and low first efficiency of the silicon-carbon composite material in the related art.

[0004] The technical solution of the present invention is as follows: The present invention provides a high first efficiency lithium-doped silicon-carbon composite material, comprising a core-shell structure consisting of a core and an outer shell, wherein the core is lithium-silicon doped porous carbon, and the outer shell is heteroatom-doped amorphous carbon.

[0005] As a further technical solution, the shell is 1% to 5% of the weight of the lithium-doped silicon-carbon composite material.

[0006] The present invention also proposes a method for preparing a high first efficiency lithium-doped silicon-carbon composite material, comprising the following steps: S1, placing porous carbon in a first reaction kettle, introducing mixed gas I, and performing vapor deposition to obtain lithium-doped porous carbon; S2, placing lithium-doped porous carbon in a second reaction kettle, introducing mixed gas II, and then introducing unsaturated hydrocarbon gas for passivation; S3, introducing mixed gas III for deposition to obtain a lithium-doped silicon-carbon composite material; The mixed gas I is composed of lithium hydride gas and heteroatom gas I; The mixed gas II is a silane mixed gas; The mixed gas III is composed of hydrocarbons and heteroatom gas II.

[0007] As a further technical solution, the heteroatom gas I and the heteroatom gas II each independently include one of boron hydride, ammonia, phosphine, and hydrogen sulfide.

[0008] As a further technical solution, the unsaturated hydrocarbon gas includes one of acetylene, propyne, butyne and ethylene.

[0009] As a further technical solution, the hydrocarbon includes one of methane, ethane, propane, and cyclopropane.

[0010] As a further technical solution, the volume ratio of lithium hydride gas to heteroatom gas in the mixed gas I is 1~5:1.

[0011] As a further technical solution, the flow rate of the mixed gas I is 100~500mL / min, and the introduction time is 30~300min.

[0012] As a further technical solution, the volume ratio of hydrocarbons to heteroatom gas II in the mixed gas III is 10:1-5.

[0013] As a further technical solution, the flow rate of the mixed gas III is 10-100 mL / min, and the introduction time is 60-600 min.

[0014] As a further technical solution, the porous carbon has an average pore size of 1 to 10 nm, an average particle size D50 of 5 to 8 μm, and a pore volume of 0.6 to 1.2 cm 3 / g, specific surface area is 1000~2000m 2 / g.

[0015] As a further technical solution, the temperature of the reactor is 900-1200°C when the mixed gas I is introduced.

[0016] As a further technical solution, the pressure of the reactor during lithium deposition is 0.1-0.5 MPa.

[0017] As a further technical solution, the temperature of the reactor is 400-600°C when the silane mixed gas is introduced.

[0018] As a further technical solution, the silane mixed gas consists of silane and nitrogen in a volume ratio of 1:9.

[0019] As a further technical solution, the flow rate of the silane mixed gas is 100~500mL / min.

[0020] As a further technical solution, the silane mixed gas is introduced for 60 to 600 minutes.

[0021] As a further technical solution, the temperature of the reactor is 500-700°C when the unsaturated hydrocarbon gas is introduced.

[0022] As a further technical solution, the flow rate of the unsaturated hydrocarbon gas is 100~500mL / min.

[0023] As a further technical solution, the unsaturated hydrocarbon gas is introduced for 60 to 600 minutes.

[0024] As a further technical solution, the temperature of the reactor is 700-900°C when the mixed gas III is introduced.

[0025] The working principle and beneficial effects of the present invention are: In the present invention, lithium hydride is deposited in porous carbon by vapor deposition and cracked to generate lithium-doped porous carbon, thereby improving the electronic conductivity of the material. Furthermore, heteroatoms are deposited in the porous carbon, and doping with non-metallic elements can improve the electronic conductivity of the material. Furthermore, the synergistic effect between the lithium metal element and the non-metallic element doped in the material can be exerted to improve the electronic conductivity of the material and reduce the defects of the porous carbon itself, thereby improving the first efficiency. Unsaturated hydrocarbons and saturated hydrocarbons are used to deposit amorphous carbon and heteroatoms on the surface of the shell by vapor deposition to improve the coating integrity of the shell, restrain the expansion of the silicon core during the charge and discharge process, and improve the cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0027] Figure 1 This is a SEM image of the lithium-doped silicon-carbon composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1 S1. 100 g of porous carbon substrate (average pore size 6 nm, average particle size D50 5.6 µm, pore volume 0.71 cm 3 / g, specific surface area is 1692m 2 / g) was placed in a fluidized bed, heated to 1000°C, evacuated to -0.009MPa, and then lithium hydride gas and ammonia gas (volume ratio, lithium hydride gas: ammonia gas = 3:1) were introduced, the chamber pressure was maintained at 0.3MPa, and the flow rate was 300mL / min for 120min to deposit lithium in the porous carbon to obtain lithium-doped porous carbon; S2. 100 g of lithium-doped porous carbon was transferred to a rotary kiln, heated to 500°C, and introduced a silane mixed gas (volume ratio, silane: nitrogen = 1:9) at a flow rate of 300 mL / min for 300 min. Then, the temperature was raised to 600°C, and acetylene gas was introduced at a flow rate of 300 mL / min for 300 min for passivation. S3. The temperature was raised to 800°C again, and a mixed gas of methane and ammonia (volume ratio, methane: ammonia = 10:3) was introduced at a flow rate of 50 mL / min for 300 minutes to obtain a lithium-doped silicon-carbon composite material.

[0030] Example 2 S1. 100 g of porous carbon substrate (average pore size 2 nm, average particle size D50 5 µm, pore volume 0.6 cm 3 / g, specific surface area is 2000m 2 / g) was placed in a fluidized bed, heated to 900°C, evacuated to -0.009MPa, and then lithium hydride gas and phosphine gas (volume ratio, lithium hydride gas:phosphine gas = 1:1) were introduced, the chamber pressure was maintained at 0.1MPa, and the flow rate was 100mL / min for 300min to deposit lithium in the porous carbon to obtain lithium-doped porous carbon; S2. 100 g of lithium-doped porous carbon was transferred to a rotary kiln, heated to 400°C, and introduced a silane mixed gas (volume ratio, silane: nitrogen = 1:9) at a flow rate of 100 mL / min for 600 min. Then, the temperature was raised to 500°C, and propyne gas was introduced at a flow rate of 100 mL / min for 600 min for passivation; S3. The temperature was raised to 700°C again, and a mixed gas of ethane and phosphine (volume ratio, ethane:phosphine = 10:1) was introduced at a flow rate of 10 mL / min for 600 min to obtain a lithium-doped silicon-carbon composite material.

[0031] Example 3 S1. 100 g of porous carbon substrate (average pore size 10 nm, average particle size D50 8 µm, pore volume 1.2 cm 3 / g, specific surface area is 1000m 2 / g) was placed in a fluidized bed, heated to 1200°C, evacuated to -0.009MPa, and then lithium hydride gas and borohydride gas (volume ratio, lithium hydride: borohydride gas = 5:1) were introduced, the chamber pressure was maintained at 0.5MPa, and the flow rate was 500mL / min for 30min to deposit lithium in the porous carbon to obtain lithium-doped porous carbon; S2. 100 g of lithium-doped porous carbon was transferred to a rotary kiln, heated to 600°C, and introduced a silane mixed gas (volume ratio, silane: nitrogen = 1:9) at a flow rate of 500 mL / min for 60 min. The temperature was then raised to 700°C, and ethylene gas was introduced at a flow rate of 500 mL / min for 60 min for passivation. S3. The temperature was raised to 900°C again, and a mixed gas of cyclopropane and hydrogen sulfide (volume ratio, cyclopropane: hydrogen sulfide = 10:5) was introduced at a flow rate of 100 mL / min for 60 minutes to obtain a lithium-doped silicon-carbon composite material.

[0032] Comparative Example 1 S1. 100 g of porous carbon substrate (average pore size 6 nm, average particle size D50 5.6 µm, pore volume 0.71 cm 3 / g, specific surface area is 1692m 2 / g) was transferred to a rotary kiln, heated to 500°C, and introduced with a silane mixed gas (volume ratio, silane: nitrogen = 1:9) at a flow rate of 300 mL / min for 300 min, then heated to 600°C, and introduced with acetylene gas at a flow rate of 300 mL / min for 300 min for passivation; S2. The temperature was raised to 800°C, and a mixed gas of methane and ammonia (volume ratio, methane: ammonia = 10:3) was introduced at a flow rate of 50 mL / min for 300 minutes to obtain a silicon-carbon composite material.

[0033] Comparative Example 2 S1. 100 g of porous carbon substrate (average pore size 6 nm, average particle size D50 5.6 µm, pore volume 0.71 cm 3 / g, specific surface area is 1692m 2 / g) was placed in a fluidized bed, heated to 1000°C, evacuated to -0.009MPa, and then lithium hydride gas and ammonia gas (volume ratio, lithium hydride gas: ammonia gas = 3:1) were introduced, the chamber pressure was maintained at 0.3MPa, and the flow rate was 300mL / min for 120min to deposit lithium in the porous carbon to obtain lithium-doped porous carbon; S2. Transfer 100 g of lithium-doped porous carbon to a rotary kiln, heat it to 500°C, introduce a silane mixed gas (volume ratio, silane: nitrogen = 1:9) at a flow rate of 300 mL / min for 300 min, then heat it to 600°C, introduce acetylene gas at a flow rate of 300 mL / min for 300 min for passivation to obtain a lithium-doped silicon-carbon composite material.

[0034] Comparative Example 3 S1. 100 g of porous carbon substrate (average pore size 6 nm, average particle size D50 5.6 µm, pore volume 0.71 cm 3 / g, specific surface area is 1692m 2 / g) was placed in a fluidized bed, heated to 1000°C, evacuated to -0.009MPa, and then lithium hydride gas and ammonia gas (volume ratio, lithium hydride gas: ammonia gas = 3:1) were introduced, the chamber pressure was maintained at 0.3MPa, and the flow rate was 300mL / min for 120min to deposit lithium in the porous carbon to obtain lithium-doped porous carbon; S2. Transfer 100 g of lithium-doped porous carbon to a rotary furnace, raise the temperature to 500°C, introduce a silane mixed gas (volume ratio, silane: nitrogen = 1:9) at a flow rate of 300 mL / min for 300 minutes, then raise the temperature to 800°C, and simultaneously introduce a methane and ammonia mixed gas (volume ratio, methane: ammonia = 10:3) at a flow rate of 50 mL / min for deposition for 300 minutes to obtain a lithium-doped silicon-carbon composite material.

[0035] Test example (1) SEM test Figure 1 This is a SEM image of the lithium-doped silicon-carbon composite material prepared in Example 1. Figure 1 It can be seen that the lithium-doped silicon-carbon composite material presents a granular structure with a particle size of about 5 μm and a smooth surface without pores, indicating that the deposition and coating integrity of the lithium-doped silicon-carbon composite material is high.

[0036] (2) Physical and chemical properties test: Referring to the national standard GB / T 38823-2020 "Silicon Carbon", the specific surface area and tap density of the lithium-doped silicon-carbon composite materials in Examples 1 to 3 and Comparative Examples 1 to 3 were tested, and the conductivity of each composite material was tested by a four-probe tester. At the same time, the gas production of the powder material was tested (100g of the powder material was placed in boiling water at 45°C, left to stand for 48 hours, and its gas production was tested); the pore size and pore volume of the lithium-doped silicon-carbon composite materials or silicon-carbon composite materials in Examples 1 to 3 and Comparative Examples 1 to 3 were also tested respectively; the test results are shown in Table 1 below.

[0037] (3) Button battery test: The lithium-doped silicon-carbon composite materials or silicon-carbon composite materials corresponding to Examples 1 to 3 and Comparative Examples 1 to 3 were used as negative electrode materials for lithium-ion batteries, and button batteries were prepared according to the following method: a binder, a conductive agent and a solvent were added to the corresponding silicon-carbon composite materials, the mixture was stirred to make a slurry, and the mixture was coated on a copper foil, and the negative electrode sheet was obtained by drying and rolling; the binder used was LA136D, the conductive agent was SP (conductive carbon black), the solvent was NMP, and the proportion of the negative electrode material, SP, LA136D and NMP was 90g:1g:9g:250mL; the electrolyte was LiPF 6 The electrolyte solution has a concentration of 1 mol / L, wherein the solvent is a mixture of EC and DEC in a volume ratio of 1:1; the metal lithium sheet is the counter electrode, and the diaphragm is a polypropylene (PP) film. Each button cell is assembled in an argon-filled glove box, and then the electrochemical performance is tested, specifically on a Wuhan Blue Electric CT2001A battery tester, with a charge and discharge voltage range of 0.005V to 2.0V and a charge and discharge rate of 0.1C; the test results are shown in Table 1 below.

[0038] The negative electrode sheet of the above button battery was also tested for full charge expansion. The specific test process is: the thickness D1 of the negative electrode sheet of the button battery after rolling was tested, and then the full charge thickness D2 of the negative electrode sheet of the button battery was dissected when it was fully charged to 100% SOC, and then the expansion rate was calculated (expansion rate = (D1-D2) / D1*100%); the test results are shown in Table 1 below.

[0039] Table 1 Test results of Examples 1 to 3 and Comparative Examples 1 to 3

[0040] It can be seen from the data in Table 1 above that the specific capacity, first efficiency and powder conductivity of the lithium-doped silicon-carbon composite materials prepared in Examples 1 to 3 are significantly better than those in Comparative Examples 1 to 3; the reason may be that: by doping lithium into the mesoporous carbon, the electronic conductivity of the material is improved and the defects of the material are reduced, the first efficiency and powder conductivity are improved, and the secondary coating and passivation of the material are achieved by depositing heteroatom-doped amorphous carbon, the coating integrity is improved and the gas production is reduced.

[0041] (4) Soft pack performance test: The lithium-doped silicon-carbon composite material or the silicon-carbon composite material doped with 95% artificial graphite corresponding to Examples 1 to 3 and Comparative Examples 1 to 3 is used as the negative electrode material (i.e., the negative electrode plate) and the positive electrode ternary material (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 ), electrolyte and diaphragm are assembled into a 5Ah soft pack battery; the diaphragm is celegard 2400, the electrolyte is LiPF6 Solution (solvent is a mixed solution of EC and DEC with a volume ratio of 1:1, LiPF 6 The concentration is 1.3 mol / L) to prepare a soft-pack battery.

[0042] The following performance tests are performed on each soft pack battery: a. Cycle performance test: Carrying out cycle performance test and rate test on each prepared soft pack battery; The test conditions for the cycle performance test are as follows: the charge and discharge voltage range is 2.5 to 4.2 V, the temperature is 25 ± 3.0 ° C, the charge and discharge rate is 1.0 C / 1.0 C, and the number of cycles is 500 times; the test results are shown in Table 2 below.

[0043] b. The test conditions for the rate test are: The battery was tested for room temperature charging DCR at different SOCs (10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%) at 3C. The test results are shown in Table 3 below.

[0044] Table 2 Test results of Examples 1 to 3 and Comparative Examples 1 to 3

[0045] It can be seen from Table 2 that the cycle performance of the soft-pack lithium-ion battery prepared by using the lithium-doped silicon-carbon composite material provided by Examples 1 to 3 is significantly better than that of Comparative Examples 1 to 3. The reason may be that: the lithium-doped silicon-carbon composite material in Examples 1 to 3 has a high specific surface area and low full-charge expansion, which improves the cycle performance; at the same time, the lithium doped in the lithium-doped silicon-carbon composite material reduces the lithium ions consumed in forming the SEI film during the charging and discharging process, thereby improving the cycle performance.

[0046] Table 3 Test results of Examples 1 to 3 and Comparative Examples 1 to 3

[0047] It can be seen from Table 3 that Examples 1 to 3 have lower charging DCR than Comparative Examples 1 to 3, and the reason may be that the lithium-doped silicon-carbon composite materials of Examples 1 to 3 are doped with metallic lithium to reduce the resistivity of the powder and the outer layer of the heteroatom-doped amorphous material reduces the interface impedance, reduces the DCR, and improves the fast charging performance of the material.

[0048] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A high first efficiency lithium-doped silicon-carbon composite material, characterized in that: The invention comprises a core-shell structure consisting of a core and an outer shell, wherein the core is lithium-silicon doped porous carbon, and the outer shell is heteroatom doped amorphous carbon.

2. The high first efficiency lithium-doped silicon-carbon composite material according to claim 1, characterized in that: The shell is 1% to 5% of the weight of the lithium-doped silicon-carbon composite material.

3. The method for preparing a high first efficiency lithium-doped silicon-carbon composite material according to any one of claims 1 to 2, characterized in that: The following steps are involved: S1, placing porous carbon in a first reaction kettle, introducing mixed gas I, and performing vapor deposition to obtain lithium-doped porous carbon; S2, placing lithium-doped porous carbon in a second reaction kettle, introducing mixed gas II, and then introducing unsaturated hydrocarbon gas for passivation; S3, introducing mixed gas III for deposition to obtain a lithium-doped silicon-carbon composite material; The mixed gas I is composed of lithium hydride gas and heteroatom gas I; The mixed gas II is a silane mixed gas; The mixed gas III is composed of hydrocarbons and heteroatom gas II.

4. The method for preparing a high first efficiency lithium-doped silicon-carbon composite material according to claim 3, characterized in that: The heteroatom gas I and the heteroatom gas II each independently include one of boron hydride, ammonia, phosphine and hydrogen sulfide.

5. The method for preparing a high first efficiency lithium-doped silicon-carbon composite material according to claim 3, characterized in that: The unsaturated hydrocarbon gas includes one of acetylene, propyne, butyne and ethylene.

6. The method for preparing a high first efficiency lithium-doped silicon-carbon composite material according to claim 3, characterized in that: The hydrocarbon includes one of methane, ethane, propane and cyclopropane.

7. The method for preparing a high first efficiency lithium-doped silicon-carbon composite material according to claim 3, characterized in that: The volume ratio of lithium hydride gas to heteroatom gas in the mixed gas I is 1-5:

1.

8. The method for preparing a high first efficiency lithium-doped silicon-carbon composite material according to claim 3, characterized in that: The flow rate of the mixed gas I is 100-500 mL / min, and the introduction time is 30-300 min.

9. The method for preparing a high first efficiency lithium-doped silicon-carbon composite material according to claim 3, characterized in that: The volume ratio of hydrocarbons to heteroatom gas II in the mixed gas III is 10:1-5.

10. The method for preparing a high first efficiency lithium-doped silicon-carbon composite material according to claim 3, characterized in that: The flow rate of the mixed gas III is 10-100 mL / min, and the introduction time is 60-600 min.

Citation Information

Cited By

  • Preparation method and application of petroleum coke-based porous carbon composite material

    CN121377015A

  • Negative electrode active material, preparation method thereof and lithium ion battery

    CN121394372A